MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC CYCOLAC™ BDT5510 ABS (Americas)
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: Automotive. High heat resistance, low gloss, color concentratable for interior applications. Natural only.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.05 g/cc1.05 g/ccASTM D792
Viscosity 1630 cP
@Shear Rate 1000 1/s,
Temperature 260 °C
1630 cP
@Shear Rate 1000 1/s,
Temperature 500 °F
melt; ASTM D3825
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow  6.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
6.0 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 14 g/10 min
@Load 10.0 kg,
Temperature 220 °C
14 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
Spiral Flow 73.7 cm29.0 in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 43.0 MPa6240 psi50 mm/min; ISO 527
 53.0 MPa7690 psi5 mm/min; ASTM D638
Tensile Modulus 2.27 GPa329 ksi5 mm/min; ASTM D638
 2.93 GPa425 ksi1mm/min; ISO 527
Flexural Yield Strength 67.0 MPa9720 psi2 mm/min; ISO 178
 81.0 MPa11700 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.03 GPa294 ksi2 mm/min; ISO 178
 2.46 GPa357 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 2.93 J/cm5.49 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 12.0 kJ/m²5.71 ft-lb/in²80*10*4; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 1.30 J/cm²6.19 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Falling Dart Impact 35.0 J25.8 ft-lbASTM D3029
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 135 µm/m-°C
@Temperature -40.0 - 60.0 °C
75.0 µin/in-°F
@Temperature -40.0 - 140 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 95.0 °C203 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 92.0 °C
@Thickness 3.20 mm
198 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 83.0 °C181 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 81.0 °C
@Thickness 3.20 mm
178 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 98.0 °C208 °FRate B/50; ISO 306
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0598 in
UL 94
 
Optical PropertiesMetricEnglishComments
Gloss 25 %25 %60°; ASTM D523
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 230 - 275 °C446 - 527 °FInjection Molding
Zone 1 195 - 240 °C383 - 464 °F
Zone 2 210 - 250 °C410 - 482 °F
Zone 3 220 - 255 °C428 - 491 °F
Melt Temperature 230 - 275 °C446 - 527 °F
Mold Temperature 50.0 - 80.0 °C122 - 176 °F
Drying Temperature 90.0 - 95.0 °C194 - 203 °FInjection Molding
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Moisture Content 0.10 %0.10 %
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 50 - 70 %50 - 70 %
Vent Depth 0.00380 - 0.00510 cm0.00150 - 0.00201 in
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI10001 / 243468

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.