MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ITW Insulcast® RTVS 27 FC Silicone Potting/Encapsulation Compound
Categories: Polymer; Thermoset; Silicone; Silicone, RTV, Encapsulation Grade

Material Notes: Insulcast® solutions are compounds designed for potting and encapsulating. INSULCAST RTVS 27 FC is a low viscosity UL 94V-0 Flame Retardant, general purpose, reversion resistant RTV Silicone. With the ability to cure rapidly at room temperature, RTVS 27 FC combines the virtues of low temperature flexibility, excellent electrical properties, high temperature resistance and easy removal for component replacement or repair.

Information provided by ITW Performance Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.50 g/cc1.50 g/ccUncured. Part A
 1.50 g/cc1.50 g/ccUncured. Part B
Viscosity 2800 cP2800 cPPart B; ASTM D1084
 2900 cP2900 cPMixed, Part A, Part B; ASTM D1084
 3000 cP3000 cPPart A; ASTM D1084
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6060ASTM D2240
Tensile Strength 3.45 MPa500 psiASTM D412
Elongation at Break 135 %135 %ASTM D412
Tear Strength 3.16 kN/m18.0 pliDie B; ASTM D624
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D257
Dielectric Constant 3.0
@Frequency 1000 Hz
3.0
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 21.7 kV/mm550 kV/inASTM D149
Dissipation Factor 0.00400.0040ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 220 µm/m-°C122 µin/in-°F
Thermal Conductivity 0.310 W/m-K2.15 BTU-in/hr-ft²-°FASTM D5470
Maximum Service Temperature, Air 204 °C399 °F
Minimum Service Temperature, Air -55.0 °C-67.0 °F
Glass Transition Temp, Tg -52.0 °C-61.6 °Fcured
 
Processing PropertiesMetricEnglishComments
Cure Time 60.0 min
@Temperature 25.0 °C
1.00 hour
@Temperature 77.0 °F
Tack-Free Time 30.0 min0.500 hourUncured. Part A, Part B
Pot Life <= 5.00 min<= 5.00 minPart A, Part B
Gel Time 3.00 - 5.00 min3.00 - 5.00 minuncured. Part A, Part B
Shelf Life 12.0 Month12.0 MonthPart A, Part B
 
Descriptive Properties
ColorBuff (Neutral)part B, uncured
 Dark Graypart A, uncured
Mix Ratio by volume1:1Part A: Part B
Mix Ratio by weight1:1Part A: Part B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PITWIN9117 / 239627

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.