MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company RTP 2107 Z  Polyetherimide (PEI) Glass Fiber 40% - FDA Type  (discontinued **)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI); Polyetherimide (PEI), 40% Glass Fiber

Material Notes: Glass Fiber 40% - FDA Type

Comments:

  • Glass Fiber
  • FDA Compliant

Unless otherwise specified, all data listed is for natural or black colored materials. Pigments can affect properties.

Information provided by RTP Company.


Data for this product has not been recently verified, please contact RTP Company for more information before specifying this grade.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.59 g/cc1.59 g/ccASTM D792
Filler Content 40 %40 %
Water Absorption 0.18 %0.18 %24 hours at 23°C; ASTM D570
Linear Mold Shrinkage  0.0010 cm/cm
@Thickness 3.17 mm
0.0010 in/in
@Thickness 0.125 in
ASTM D955
 0.0020 cm/cm
@Thickness 6.35 mm
0.0020 in/in
@Thickness 0.250 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 123123ASTM D785
Tensile Strength, Ultimate 200 MPa29000 psiASTM D638
Elongation at Break 2.0 - 3.0 %2.0 - 3.0 %ASTM D638
Modulus of Elasticity 13.8 GPa2000 ksiASTM D638
Flexural Yield Strength 283 MPa41000 psiASTM D790
Flexural Modulus 11.0 GPa1600 ksiASTM D790
Compressive Yield Strength 155 MPa22500 psiASTM D695
Izod Impact, Notched 1.01 J/cm
@Thickness 3.17 mm
1.90 ft-lb/in
@Thickness 0.125 in
ASTM D256
Izod Impact, Unnotched 6.41 J/cm
@Thickness 3.17 mm
12.0 ft-lb/in
@Thickness 0.125 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Dielectric Constant 4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
Dry; ASTM D150
Dielectric Strength >= 19.7 kV/mm>= 500 kV/inS/T; ASTM D149
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
Dry; ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 21.6 µm/m-°C
@Temperature 20.0 °C
12.0 µin/in-°F
@Temperature 68.0 °F
ASTM D696
Thermal Conductivity 0.259 W/m-K1.80 BTU-in/hr-ft²-°FThrough-plane; ASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 213 °C415 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °FASTM D648
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
Per testing by RTP Company; ASTM D3801
 
Processing PropertiesMetricEnglishComments
Processing Temperature 349 - 382 °C660 - 720 °F
Mold Temperature 135 - 177 °C275 - 350 °F
Injection Pressure 82.7 - 124 MPa12000 - 18000 psi
 
Compliance PropertiesMetricEnglishComments
FDA YesYes
 
Descriptive Properties
ColorNatural/Black

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PR4934 / 64269

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.