MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Corning LXP GREEN Tinted Optical Glass
Categories: Ceramic; Glass; Optical

Material Notes: Application : 100 % UV absorbing glass suited for general or special purpose Tinted glass. Pass cited standards for traffic signal recognition at 1.8 mm thickness

Information provided by Corning Incorporated.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.50 g/cc0.0903 lb/in³
 
Thermal PropertiesMetricEnglishComments
CTE, linear 8.60 µm/m-°C4.78 µin/in-°F
Softening Point 703 °C1300 °F
Annealing Point 528 °C982 °F
Strain Point 703 °C1300 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.523
@Wavelength 587.6 nm
1.523
@Wavelength 587.6 nm
Line: d; Helium
Transmission, Visible  10 %
@Wavelength 380 - 500 nm,
Thickness 1.80 mm
10 %
@Wavelength 380 - 500 nm,
Thickness 0.0709 in
Blue light transmission factor
 15 %
@Wavelength 380 - 780 nm,
Thickness 1.80 mm
15 %
@Wavelength 380 - 780 nm,
Thickness 0.0709 in
Luminous
IR Transmittance 1.0 %
@Wavelength 780 - 2000 nm,
Thickness 2.00 mm
1.0 %
@Wavelength 780 - 2000 nm,
Thickness 0.0787 in
Solar
UV Transmittance  <= 0.10 %
@Wavelength 280 - 315 nm,
Thickness 1.80 mm
<= 0.10 %
@Wavelength 280 - 315 nm,
Thickness 0.0709 in
UV - B t?(max)
 <= 0.10 %
@Wavelength 280 - 315 nm,
Thickness 1.80 mm
<= 0.10 %
@Wavelength 280 - 315 nm,
Thickness 0.0709 in
t(avg)
 <= 0.10 %
@Wavelength 315 - 350 nm,
Thickness 1.80 mm
<= 0.10 %
@Wavelength 315 - 350 nm,
Thickness 0.0709 in
Solar UV-B transmission factor
 <= 0.10 %
@Wavelength 315 - 350 nm,
Thickness 1.80 mm
<= 0.10 %
@Wavelength 315 - 350 nm,
Thickness 0.0709 in
UV - A t?(max)
 <= 0.50 %
@Wavelength 380 - 500 nm,
Thickness 1.80 mm
<= 0.50 %
@Wavelength 380 - 500 nm,
Thickness 0.0709 in
t(avg)
 <= 0.50 %
@Wavelength 380 - 500 nm,
Thickness 1.80 mm
<= 0.50 %
@Wavelength 380 - 500 nm,
Thickness 0.0709 in
Solar UV-A transmission factor
 
Descriptive Properties
ColorGreen

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Saint-Gobain Korel® K20 Very Soft Micro-cellular Polyurethane Foam
Silberline Sparkle Silver® 3141-ST
Schott ZERODUR® K20 Glass Ceramic
Morgan Advanced Ceramics Green Glass Paper Thermal Ceramic

CCORN918 / 233329

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.