MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Parker Chomerics CHO-FAB CRS Shielding Tape
Categories: Polymer; Adhesive; Tape

Material Notes: Conductive Adhesive Nickel-Plated Fabric

Description: CHO-FAB® tape is a corrosion resistant nickel-plated cloth coated with Chomerics’ highly conductive pressure-sensitive adhesive. CHO-FAB® tape is extremely strong and lightweight, and has excellent conformability/wrapability to enhance shielding performance and appearance. Use of corrosion resistant nickel-plated cloth and Chomerics’ superior metal-particle-filled conductive adhesive technology produces a tape used in a wide variety of EMI shielding and grounding applications.

Typical Applications: Provide a low impedance connection between a braided cable shield and the metal connector backshell in molded cables. An effective EMI shielded assembly can be achieved without soldering the tape to the braid or backshell; EMI radiation measurement troubleshooting, using CHO-FOIL tape to shield ventilation slots or seam gaps; Provide electrical continuity in seams of EMI shielded rooms and electronic enclosures; Supply electrical contact to surfaces that can’t be soldered to, such as conductive plastic or aluminum; EMI shield for cables by wrapping the tape around the cable. An overlap is recommended; ESD shielding; Provide corrosion-resistant ground contact points; Fabric tape available where weight and flexibility are important, such as for wrapping cables.

Information provided by Chomerics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Thickness 38.1 microns1.50 milAdhesive thickness
 102 microns4.00 milFabric thickness
 140 microns5.50 milTotal
 
Mechanical PropertiesMetricEnglishComments
Peel Strength 0.491 kN/m2.80 pliInitial; ASTM D1000
 0.508 kN/m
@Temperature 85.0 °C
2.90 pli
@Temperature 185 °F
95% RH; ASTM D1000
 0.473 kN/m
@Temperature 121 °C,
Time 605000 sec
2.70 pli
@Temperature 250 °F,
Time 168 hour
ASTM D1000
 0.649 kN/m
@Temperature 85.0 °C,
Time 605000 sec
3.70 pli
@Temperature 185 °F,
Time 168 hour
ASTM D1000
 0.368 kN/m
@Time 605000 sec
2.10 pli
@Time 168 hour
Salt fog corrosion; ASTM D1000
Taber Abrasion, mg/1000 Cycles <= 350<= 350500 gram weight. CS-10 wheel; CHO-TP-57
 
Electrical PropertiesMetricEnglishComments
Surface Resistance <= 0.10 ohm<= 0.10 ohmInitial Surface Resistivity (SR); CHO-TP-57
 <= 0.10 ohm<= 0.10 ohmInitial through resistivity (TR); CHO-TP-57
 <= 0.10 ohm<= 0.10 ohmInitial Taber Abrasion; CHO-TP-57
 <= 0.10 ohm
@Temperature 85.0 °C
<= 0.10 ohm
@Temperature 185 °F
95% RH; (SR); CHO-TP-57
 <= 0.15 ohm
@Temperature 85.0 °C
<= 0.15 ohm
@Temperature 185 °F
95% RH; (TR); CHO-TP-57
 <= 0.10 ohm
@Temperature 85.0 °C,
Time 605000 sec
<= 0.10 ohm
@Temperature 185 °F,
Time 168 hour
(SR); CHO-TP-57
 <= 0.10 ohm
@Temperature 121 °C,
Time 605000 sec
<= 0.10 ohm
@Temperature 250 °F,
Time 168 hour
(SR); CHO-TP-57
 <= 0.15 ohm
@Temperature 121 °C,
Time 605000 sec
<= 0.15 ohm
@Temperature 250 °F,
Time 168 hour
(TR); CHO-TP-57
 <= 0.15 ohm
@Temperature 85.0 °C,
Time 605000 sec
<= 0.15 ohm
@Temperature 185 °F,
Time 168 hour
(TR); CHO-TP-57
 <= 0.10 ohm
@Time 605000 sec
<= 0.10 ohm
@Time 168 hour
Salt fog corrosion; (SR); CHO-TP-57
 <= 1.0 ohm
@Time 605000 sec
<= 1.0 ohm
@Time 168 hour
Salt fog corrosion; (TR); CHO-TP-57
Surface Resistivity per Square <= 0.10 ohm<= 0.10 ohm[ohm/in2]; <.016 ohm/cm2; MIL-STD-202C
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 82.0 °C180 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Descriptive Properties
Adhesion to Aluminum>40 oz./inchASTM D1000
Adhesive TypeElectrically Conductive, Pressure-Sensitive Acrylic
Foil/Fabric TypeNickel-Plated Fabric

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Parker Chomerics CHO-FAB CFT Shielding Tape
ArcelorMittal MartINsite® 1500 Cold Rolled Steel
ArcelorMittal MartINsite® 1200 Cold Rolled Steel
ArcelorMittal FF 280 D Very High Strength Cold Rolled Steel
ArcelorMittal Complex Phase Steel 1000 Y800 Very High Strength Cold Rolled Steel

PCHOME070 / 28292

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.