Physical Properties | Metric | English | Comments |
---|
Density | 3.51 g/cc | 0.127 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 560 | 560 |
Modulus of Elasticity | 84.0 GPa | 12200 ksi |
Modulus of Rupture | 0.0439 GPa | 6.37 ksi |
Poissons Ratio | 0.29 | 0.29 |
Shear Modulus | 35.4 GPa | 5130 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 3.20e+10 ohm-cm @Temperature 550 °C | 3.20e+10 ohm-cm @Temperature 1020 °F |
| 3.20e+12 ohm-cm @Temperature 450 °C | 3.20e+12 ohm-cm @Temperature 842 °F |
| 7.90e+14 ohm-cm @Temperature 350 °C | 7.90e+14 ohm-cm @Temperature 662 °F |
Dielectric Constant | 9.95 @Frequency 100 - 10000 Hz, Temperature 350 °C | 9.95 @Frequency 100 - 10000 Hz, Temperature 662 °F |
| 10.05 @Frequency 10000 Hz, Temperature 400 °C | 10.05 @Frequency 10000 Hz, Temperature 752 °F |
| 10.08 @Frequency 100 Hz, Temperature 400 °C | 10.08 @Frequency 100 Hz, Temperature 752 °F |
| 10.08 @Frequency 1000 Hz, Temperature 400 °C | 10.08 @Frequency 1000 Hz, Temperature 752 °F |
| 10.35 @Frequency 10000 Hz, Temperature 550 °C | 10.35 @Frequency 10000 Hz, Temperature 1020 °F |
| 10.41 @Frequency 1000 Hz, Temperature 550 °C | 10.41 @Frequency 1000 Hz, Temperature 1020 °F |
| 10.61 @Frequency 100 Hz, Temperature 550 °C | 10.61 @Frequency 100 Hz, Temperature 1020 °F |
Dissipation Factor | 0.00115 @Frequency >=100 Hz, Temperature 300 °C | 0.00115 @Frequency >=100 Hz, Temperature 572 °F |
| 0.0013 @Frequency >=1000 Hz, Temperature 3200 °C | 0.0013 @Frequency >=1000 Hz, Temperature 5790 °F |
| 0.00137 @Frequency >=100 Hz, Temperature 25.0 °C | 0.00137 @Frequency >=100 Hz, Temperature 77.0 °F |
| 0.00137 @Frequency >=1000 Hz, Temperature 25.0 °C | 0.00137 @Frequency >=1000 Hz, Temperature 77.0 °F |
| 0.0015 @Frequency >=10000 Hz, Temperature 300 °C | 0.0015 @Frequency >=10000 Hz, Temperature 572 °F |
| 0.0017 @Frequency >=10000 Hz, Temperature 25.0 °C | 0.0017 @Frequency >=10000 Hz, Temperature 77.0 °F |
| 0.0039 @Frequency >=10000 Hz, Temperature 550 °C | 0.0039 @Frequency >=10000 Hz, Temperature 1020 °F |
| 0.013 @Frequency >=1000 Hz, Temperature 550 °C | 0.013 @Frequency >=1000 Hz, Temperature 1020 °F |
| 0.072 @Frequency >=100 Hz, Temperature 550 °C | 0.072 @Frequency >=100 Hz, Temperature 1020 °F |
|
Thermal Properties | Metric | English | Comments |
---|
Thermal Conductivity | 1.00 W/m-K | 6.94 BTU-in/hr-ft²-°F |
| 2.01 W/m-K @Temperature 190 °C | 13.9 BTU-in/hr-ft²-°F @Temperature 374 °F |
| 3.01 W/m-K @Temperature 320 °C | 20.9 BTU-in/hr-ft²-°F @Temperature 608 °F |
| 4.02 W/m-K @Temperature 425 °C | 27.8 BTU-in/hr-ft²-°F @Temperature 797 °F |
| 5.02 W/m-K @Temperature 525 °C | 34.8 BTU-in/hr-ft²-°F @Temperature 977 °F |
| 6.02 W/m-K @Temperature 600 °C | 41.7 BTU-in/hr-ft²-°F @Temperature 1110 °F |
Maximum Service Temperature, Air | 650 °C | 1200 °F |
| 850 °C | 1560 °F |
Softening Point | 874 °C | 1610 °F |
Annealing Point | 735 °C | 1360 °F |
Strain Point | 697 °C | 1290 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.56569 @Wavelength 5500 nm | 1.56569 @Wavelength 5500 nm |
| 1.59521 @Wavelength 4500 nm | 1.59521 @Wavelength 4500 nm |
| 1.61686 @Wavelength 3500 nm | 1.61686 @Wavelength 3500 nm |
| 1.63203 @Wavelength 2500 nm | 1.63203 @Wavelength 2500 nm |
| 1.6431 @Wavelength 1500 nm | 1.6431 @Wavelength 1500 nm |
| 1.6506 @Wavelength 950 nm | 1.6506 @Wavelength 950 nm |
| 1.65289 @Wavelength 850 nm | 1.65289 @Wavelength 850 nm |
| 1.65599 @Wavelength 750 nm | 1.65599 @Wavelength 750 nm |
| 1.656 @Wavelength 656.3 nm | 1.656 @Wavelength 656.3 nm |
| 1.6601 @Wavelength 589.3 nm | 1.6601 @Wavelength 589.3 nm |
| 1.66356 @Wavelength 600 nm | 1.66356 @Wavelength 600 nm |
| 1.66754 @Wavelength 550 nm | 1.66754 @Wavelength 550 nm |
| 1.6702 @Wavelength 486.1 nm | 1.6702 @Wavelength 486.1 nm |
| 1.69093 @Wavelength 400 nm | 1.69093 @Wavelength 400 nm |
Abbe Number | 46.5 | 46.5 |
Transmission, Visible | 85 % @Thickness 1.346 mm, Wavelength 400 nm | 85 % @Thickness 0.05299 in, Wavelength 400 nm |
| 86 % @Wavelength 450 - 650 nm, Thickness 1.346 mm | 86 % @Wavelength 450 - 650 nm, Thickness 0.05299 in |
IR Transmittance | 5.0 % @Thickness 1.346 mm, Wavelength 6000 nm | 5.0 % @Thickness 0.05299 in, Wavelength 6000 nm |
| 68 % @Thickness 1.346 mm, Wavelength 5000 nm | 68 % @Thickness 0.05299 in, Wavelength 5000 nm |
| 85 % @Wavelength 3000 - 4000 nm, Thickness 1.346 mm | 85 % @Wavelength 3000 - 4000 nm, Thickness 0.05299 in |
| 88 % @Wavelength 1000 - 2500 nm, Thickness 1.346 mm | 88 % @Wavelength 1000 - 2500 nm, Thickness 0.05299 in |
UV Transmittance | 0.00 % @Thickness 1.346 mm, Wavelength 250 nm | 0.00 % @Thickness 0.05299 in, Wavelength 250 nm |
| 10 % @Thickness 1.346 mm, Wavelength 300 nm | 10 % @Thickness 0.05299 in, Wavelength 300 nm |
| 70 % @Thickness 1.346 mm, Wavelength 350 nm | 70 % @Thickness 0.05299 in, Wavelength 350 nm |
|
Descriptive Properties |
---|
Stress Optical Coefficient | 262 nm/cm/kg/mm² |