MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

AGC Asahiklin AE3000ATE Solvent
Categories: Fluid; Solvent

Material Notes: Asahiklin AE3000AT, a mixture of Trans-1,-2-Dichloroethylene, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, is a non-flammable, non-ozone depleting solvent.

Applications:

  • Defluxing of printed wiring assemblies
  • Precision cleaning of plastics, substrates, electrical component, metals, and particle removal
  • Drying agent after cleaning with hydrocarbons or alcohols
  • Drying agent after aqueous cleaning
  • Replacement for HCFC, perchloroethylene, trichloroethylene, Dupont™ Vetrel® & 3M™ Novec™ solvents
Benefits:
  • Non-flammable
  • Non-corrosive
  • Superior drying property
  • Excellent permeability
  • Recyclable
  • Low global warming potential (GWP)
  • Zero ozone depletion potential (ODP)
  • No surfactants necessary
  • Recoverable by simple distillation
  • Can be used with ultrasonics
  • Material compatibility with a wide variety of metals, plastics, and elastomers
  • Excellent thermal, chemical, and hydrolytic stability
  • Low surface tension, low viscosity, high liquid density

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.35 g/cc1.35 g/cc
 1.25 g/cc
@Temperature 15.0 °C
1.25 g/cc
@Temperature 59.0 °F
 1.80 g/cc
@Temperature 35.0 °C
1.80 g/cc
@Temperature 95.0 °F
Viscosity 0.459 cP0.459 cP
 0.4851 cP
@Temperature 35.0 °C
0.4851 cP
@Temperature 95.0 °F
 0.5586 cP
@Temperature 15.0 °C
0.5586 cP
@Temperature 59.0 °F
 0.7056 cP
@Temperature -20.0 °C
0.7056 cP
@Temperature -4.00 °F
Vapor Pressure  0.490 bar
@Temperature 20.0 °C
368 torr
@Temperature 68.0 °F
 0.981 bar
@Temperature 40.0 °C
736 torr
@Temperature 104 °F
Surface Tension 18 dynes/cm18 dynes/cm
 
Thermal PropertiesMetricEnglishComments
Heat of Vaporization 200 J/g
@Temperature 39.0 °C
86.0 BTU/lb
@Temperature 102 °F
Specific Heat Capacity 1.40 J/g-°C0.335 BTU/lb-°F
Melting Point -50.0 °C-58.0 °F
Boiling Point 42.0 °C108 °F
 
Descriptive Properties
Global Warming Potential257
KB38
Material CompatibilityABSat boiling point for 5 min, 45.5% Weight Change, 23.7% Linear Swell, 0.9% Extractables
 ABSat boiling point for 3 days, 181% Weight Change, affected Linear Swell, 4.5% Extractables
 Chlorosulfonated polyethylene (CSM)at boiling point for 3 days, 32.4% Weight Change, 27% Linear Swell, 12.7% Extractables
 Chlorosulfonated polyethylene (CSM)at boiling point for 5 min, 15.2% Weight Change, 13% Linear Swell, 2.1% Extractables
 Epoxy (FR)at boiling point for 3 days, 7.4% Weight Change, 12% Linear Swell, 0.1% Extractables
 Epoxy (FR)at boiling point for 5 min, 0.4% Weight Change, 0.5% Linear Swell, <0.1% Extractables
 Ethylene propylene diene terpolymer (EPDM)at boiling point for 5 min, 16.1% Weight Change, 13.6% Linear Swell, 4.2% Extractables
 Ethylene propylene diene terpolymer (EPDM)at boiling point for 3 days, 16.7% Weight Change, 7.8% Linear Swell, 18.6% Extractables
 Fluoroelastomer E (FKM)at boiling point for 3 days, 84.2% Weight Change, 109.5% Linear Swell, 3.8% Extractables
 Fluoroelastomer E (FKM)at boiling point for 5 min, 11.1% Weight Change, 14.6% Linear Swell, <0.1% Extractables
 Isobutylene isoprene rubber (IIR)at boiling point for 5 min, 18.3% Weight Change, 15.6% Linear Swell, 3.2% Extractables
 Isobutylene isoprene rubber (IIR)at boiling point for 3 days, 38.1% Weight Change, 29% Linear Swell, 14.3% Extractables
 Natural rubber (NR)at boiling point for 5 min, 23% Weight Change, 20.9% Linear Swell, 1.3% Extractables
 Natural rubber (NR)at boiling point for 3 days, 46.7% Weight Change, 33.9% Linear Swell, 12.7% Extractables
 Nitryl rubber (NBR)at boiling point for 5 min, 29.1% Weight Change, 27% Linear Swell, 3.2% Extractables
 Nitryl rubber (NBR)at boiling point for 3 days, 66.2% Weight Change, 59.9% Linear Swell, 13.5% Extractables
 Nylon6at boiling point for 5 min, <0.1% Weight Change, -4% Linear Swell, 0.3% Extractables
 Nylon6at boiling point for 3 days, 8.5% Weight Change, 2.8% Linear Swell, 0.1% Extractables
 Nylon66at boiling point for 3 days, 7.3% Weight Change, 7.5% Linear Swell, 0.2% Extractables
 Nylon66at boiling point for 5 min, 0.2% Weight Change, -0.1% Linear Swell, 0.2% Extractables
 PCTFEat boiling point for 5 min, 0.2% Weight Change, 0.7% Linear Swell, <0.1% Extractables
 PCTFEat boiling point for 3 days, 10.4% Weight Change, 16.4% Linear Swell, <0.1% Extractables
 Phenolicat boiling point for 3 days, 11.4% Weight Change, 11.4% Linear Swell, 1.2% Extractables
 Phenolicat boiling point for 5 min, 0.2% Weight Change, 0.2% Linear Swell, <0.1% Extractables
 Polyacetalat boiling point for 5 min, 0.4% Weight Change, 0.4% Linear Swell, <0.1% Extractables
 Polyacetalat boiling point for 3 days, 11.4% Weight Change, 13.1% Linear Swell, 0.4% Extractables
 Polybutylene terephthalateat boiling point for 5 min, 1% Weight Change, 1.2% Linear Swell, <0.1% Extractables
 Polybutylene terephthalateat boiling point for 3 days, 13.5% Weight Change, 12.3% Linear Swell, 0.6% Extractables
 Polycarbonateat boiling point for 3 days, 36% Weight Change, 65.2% Linear Swell, 1% Extractables
 Polycarbonateat boiling point for 5 min, 17.2% Weight Change, 23.2% Linear Swell, 0.2% Extractables
 Polychloroprene (CR)at boiling point for 5 min, 18.7% Weight Change, 17.8% Linear Swell, <0.1% Extractables
 Polychloroprene (CR)at boiling point for 3 days, 31.8% Weight Change, 28% Linear Swell, 14.2% Extractables
 Polyester (FR)at boiling point for 5 min, 3.1% Weight Change, 3% Linear Swell, 0.2% Extractables
 Polyester (FR)at boiling point for 3 days, 76.8% Weight Change, 134.7% Linear Swell, 5.3% Extractables
 Polyethylene (HP)at boiling point for 3 days, 110.4% Weight Change, affected Linear Swell, 1.1% Extractables
 Polyethylene (HP)at boiling point for 5 min, 8.6% Weight Change, 6% Linear Swell, <0.1% Extractables
 Polyethylene (LP)at boiling point for 5 min, 1.5% Weight Change, 1.5% Linear Swell, <0.1% Extractables
 Polyethylene (LP)at boiling point for 3 days, 16.3% Weight Change, 12.8% Linear Swell, 2.4% Extractables
 Polyethylene terephthalateat boiling point for 5 min, 25.9% Weight Change, 22.2% Linear Swell, 0.3% Extractables
 Polyethylene terephthalateat boiling point for 3 days, 71.4% Weight Change, 78% Linear Swell, 2.6% Extractables
 Polyphenylene oxideat boiling point for 3 days, 107.6% Weight Change, affected Linear Swell, 10.6% Extractables
 Polyphenylene oxideat boiling point for 5 min, 34% Weight Change, 20.3% Linear Swell, 1.2% Extractables
 Polyphenylene sulfideat boiling point for 5 min, 0.1% Weight Change, -0.9% Linear Swell, <0.1% Extractables
 Polyphenylene sulfideat boiling point for 3 days, 3.8% Weight Change, 4.8% Linear Swell, 0.1% Extractables
 Polypropyleneat boiling point for 5 min, 2.4% Weight Change, 1.8% Linear Swell, 0.3% Extractables
 Polypropyleneat boiling point for 3 days, 31% Weight Change, 22.1% Linear Swell, 1% Extractables
 Polystyreneat boiling point for 3 days, affected Weight Change, affected Linear Swell, 105.8% Extractables
 Polystyreneat boiling point for 5 min, 31.2% Weight Change, 16.9% Linear Swell, 0.8% Extractables
 Polysulfide rubber FA(T)at boiling point for 5 min, 19.8% Weight Change, 16.4% Linear Swell, 1.9% Extractables
 Polysulfide rubber FA(T)at boiling point for 3 days, 63.8% Weight Change, 50.1% Linear Swell, 13.6% Extractables
 Polyvinyl chloride (plasticized)at boiling point for 5 min, 23.5% Weight Change, 19% Linear Swell, 5.8% Extractables
 Polyvinyl chloride (plasticized)at boiling point for 3 days, -7.4% Weight Change, -17.5% Linear Swell, 26.8% Extractables
 Polyvinyl chloride (rigid)at boiling point for 3 days, 43.5% Weight Change, 45% Linear Swell, 0.8% Extractables
 Polyvinyl chloride (rigid)at boiling point for 5 min, 3.8% Weight Change, 4% Linear Swell, <0.1% Extractables
 PTFEat boiling point for 5 min, 0.1% Weight Change, 0.2% Linear Swell, <0.1% Extractables
 PTFEat boiling point for 3 days, 2.6% Weight Change, 3.9% Linear Swell, 0.1% Extractables
 PTFEat boiling point for 7 days, 2.7% Weight Change, 1.1% Linear Swell, <0.1% Extractables
 Silicone rubber (Q)at boiling point for 5 min, 66.7% Weight Change, 54.8% Linear Swell, 0.5% Extractables
 Silicone rubber (Q)at boiling point for 3 days, 167% Weight Change, 128.6% Linear Swell, 2.5% Extractables
 Urethane rubber (UR)at boiling point for 3 days, 178.6% Weight Change, 129.7% Linear Swell, 13.2% Extractables
 Urethane rubber (UR)at boiling point for 5 min, 40% Weight Change, 35.8% Linear Swell, 6% Extractables
 Vitonat boiling point for 7 days, 72% Weight Change, 60.4% Linear Swell, 6.8% Extractables
 Viton (Chemical Resistant)at boiling point for 7 days, 90.5% Weight Change, 68.4% Linear Swell, 1.2% Extractables
 Viton (FDA White)at boiling point for 7 days, 57.1% Weight Change, 53.9% Linear Swell, 0.9% Extractables
 Viton (Low Temp)at boiling point for 7 days, 71.2% Weight Change, 54.6% Linear Swell, 0.2% Extractables
Material Composition1-3%Ethanol
 43-52%1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether
 56-55%Trans-1,2-dichloroethylene
Relative Evaporation Rate92Ether=100

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Polyram PlusTek PA108 Nylon6/6.6 Alloy for Injection Molding
AGC Asahiklin AE3000AT Solvent
Overview of materials for Medium Alloy Steel
Overview of materials for AISI 4000 Series Steel
Iran Petrochemical (PCC) PET BG-821 Polyethylene Terephthalate

PAGCX073 / 191182

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.