MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Hexcel® HexPly® M65 Bismaleimide Resin, Carbon Tape Form
Categories: Polymer; Thermoset; Bismaleimide (BMI)

Material Notes: Fiber: IM7-12K

Information provided by HexCel

Key Words: BMI
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.56 g/cc0.0564 lb/in³Laminate
Volatiles <= 2.0 %<= 2.0 %Prepreg
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 1579 MPa
@Temperature 23.0 °C
229000 psi
@Temperature 73.4 °F
Elongation at Yield 1.73 %
@Temperature 23.0 °C
1.73 %
@Temperature 73.4 °F
Tensile Modulus 85.4 GPa
@Temperature 23.0 °C
12400 ksi
@Temperature 73.4 °F
Flexural Yield Strength  758 MPa
@Temperature 177 °C
110000 psi
@Temperature 351 °F
IM7 (12K); [0°, 90°]5s; Wet condition
 938 MPa
@Temperature 232 °C
136000 psi
@Temperature 450 °F
IM7 (12K); [0°, 90°]5s
 1172 MPa
@Temperature 23.0 °C
170000 psi
@Temperature 73.4 °F
Flexural Modulus  90.7 GPa
@Temperature 177 °C
13200 ksi
@Temperature 351 °F
IM7 (12K); [0°, 90°]5s; Wet condition
 92.7 GPa
@Temperature 232 °C
13400 ksi
@Temperature 450 °F
IM7 (12K); [0°, 90°]5s
 94.7 GPa
@Temperature 23.0 °C
13700 ksi
@Temperature 73.4 °F
Compressive Yield Strength  181 MPa
@Temperature 23.0 °C
26300 psi
@Temperature 73.4 °F
 696 MPa
@Temperature 177 °C
101000 psi
@Temperature 351 °F
IM7 (12K); [90°, 0°]2s; Wet condition
 1048 MPa
@Temperature 232 °C
152000 psi
@Temperature 450 °F
IM7 (12K); [90°, 0°]2s
 1234 MPa
@Temperature 23.0 °C
179000 psi
@Temperature 73.4 °F
Shear Modulus  2.10 GPa
@Temperature 177 °C
305 ksi
@Temperature 351 °F
IM7 (12K); [+/- 45°]2s; In Plane; Wet condition
 3.10 GPa
@Temperature 232 °C
450 ksi
@Temperature 450 °F
IM7 (12K); [+/- 45°]2s; In Plane
 4.70 GPa
@Temperature 23.0 °C
682 ksi
@Temperature 73.4 °F
Shear Strength  41.0 MPa
@Temperature 177 °C
5950 psi
@Temperature 351 °F
IM7 (12K); [0°, 90°]5s; Short Beam; Wet condition
 58.7 MPa
@Temperature 232 °C
8510 psi
@Temperature 450 °F
IM7 (12K); [0°, 90°]5s; Short Beam
 72.0 MPa
@Temperature 177 °C
10400 psi
@Temperature 351 °F
IM7 (12K); [+/- 45°]2s; In Plane; Wet condition
 80.9 MPa
@Temperature 23.0 °C
11700 psi
@Temperature 73.4 °F
 82.0 MPa
@Temperature 232 °C
11900 psi
@Temperature 450 °F
IM7 (12K); [+/- 45°]2s; In Plane
 129 MPa
@Temperature 23.0 °C
18700 psi
@Temperature 73.4 °F
 
Descriptive Properties
Cured Thickness per Ply (cm)0.0137Laminate
Dry Resin Content (%)33Prepreg
Fiber Volume (%)59Laminate

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Vyncolit Neopreg Kinel® SK4503 S5 Aramid Reinforced Molding Compound
Hexcel® HexFlow® RTM651 One-part Modified BMI Resin
Henkel Hysol EA 9833.1 (BMI) Core Splice Adhesive
Henkel Hysol EA 9673 (BMI) Film Adhesive
Evonik Compimide® TM124-ether 2,2'-Bis(4-allyloxyphenyl)propane

PHEXC015 / 98485

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.