MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

DuPont Mobility and Materials Sorona® 3030G NC010 PTT-GF30  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polyester, TP; Polytrimethylene Terephthalate (PTT)

Material Notes: 30% Glass Reinforced Polytrimethylene Terephthalate

Information provided by DuPont.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.56 g/cc0.0564 lb/in³ISO 1183
Melt Density 1.35 g/cc
@Temperature >=227 °C
0.0488 lb/in³
@Temperature >=441 °F
Water Absorption 0.080 %
@Time 86400 sec
0.080 %
@Time 24.0 hour
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0070 cm/cm0.0070 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 165 MPa23900 psiISO 527-1/-2
Elongation at Break 2.5 %2.5 %ISO 527-1/-2
Tensile Modulus 11.0 GPa1600 ksiISO 527-1/-2
Flexural Strength 245 MPa35500 psiISO 178
Flexural Modulus 9.60 GPa1390 ksiISO 178
Poissons Ratio 0.340.34ISO 527-1/-2
Charpy Impact Unnotched  4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 5.00 J/cm²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.900 J/cm²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 0.900 J/cm²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 8.00e+13 ohm8.00e+13 ohmIEC 62631-3-2
Dielectric Constant  4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.2
@Frequency 100 Hz
4.2
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 38.0 kV/mm965 kV/inIEC 60243-1
Dissipation Factor  0.0012
@Frequency 100 Hz
0.0012
@Frequency 100 Hz
IEC 62631-2-1
 0.0155
@Frequency 1e+6 Hz
0.0155
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 350 V350 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 7.00 µm/m-°C3.89 µin/in-°FISO 11359-1/-2
 16.0 µm/m-°C
@Temperature 55.0 - 160 °C
8.89 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
 25.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
13.9 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 83.0 µm/m-°C46.1 µin/in-°FISO 11359-1/-2
 67.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
37.2 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
 120 µm/m-°C
@Temperature 55.0 - 160 °C
66.7 µin/in-°F
@Temperature 131 - 320 °F
ISO 11359-1/-2
Melting Point 227 °C441 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 226 °C439 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °FISO 75-1/-2
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
IEC 60695-11-10
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
Flame Spread 30.0 mm/min
@Thickness 1.00 mm
1.18 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 20 %20 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 270 °C482 - 518 °FInjection
 260 °C500 °FInjection Optimum
Mold Temperature 80.0 - 110 °C176 - 230 °FInjection
 100 °C212 °FInjection Optimum
Ejection Temperature 175 °C347 °FInjection
Drying Temperature 120 °C248 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.020 %0.020 %Injection
 
Descriptive Properties
AdditivesRelease agent
Back pressureAs low as possibleInjection
Delivery formPellets
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Part Marking Code>PTT-GF30<ISO 11469
ProcessingInjection Molding
Resin IdentificationPTT-GF30ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Sorona® 3030G BK001 PTT-GF30
AIM SAC305 Lead-Free Solder for Photonic Packaging
DuPont Mobility and Materials Sorona® 3015G NC010 PTT-GF15
DuPont Mobility and Materials Sorona® FG3015G NC010 PTT-GF15
DuPont Mobility and Materials Sorona® 2045G BK346A PTT-GF45

PZDSX5285 / 197925

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.