MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Techmer ES Luriblend® PA6 GF30 TL15 30% Glass Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled; Nylon 6, Heat Stabilized; Nylon 6, PTFE Filled

Material Notes: Availability: North America

Forms: Pellets

Filler/Reinforcement: Glass Fiber, 15% Filler by Weight

Additive: Heat Stabilized and PTFE Lubricant(15%)

Features: Lubricated, Good Wear Resistance, Heat Stabilized and Low Friction

Appearance: Natural Color

Information provided by TP Composites, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.49 g/cc0.0538 lb/in³ASTM D792
Water Absorption 0.95 %
@Time 86400 sec
0.95 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0040 cm/cm
@Thickness 3.17 mm
0.0040 in/in
@Thickness 0.125 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9090ASTM D785
Tensile Strength, Yield 137 MPa19800 psiASTM D638
Elongation at Break 2.0 %2.0 %ASTM D638
Flexural Strength 197 MPa28500 psiASTM D790
Flexural Modulus 8.27 GPa1200 ksiASTM D790
Izod Impact, Notched 0.801 J/cm
@Thickness 3.17 mm
1.50 ft-lb/in
@Thickness 0.125 in
ASTM D256
Coefficient of Friction, Dynamic 0.290.29ASTM D1894
Coefficient of Friction, Static 0.230.23ASTM D1894
K (wear) Factor 34.2 x 10-8 mm³/N-M17.0 x 10-10 in³-min/ft-lb-hr
Limiting Pressure Velocity 0.543 MPa-m/sec15500 psi-ft/min10 fpm
 0.578 MPa-m/sec16500 psi-ft/min1000 fpm
 0.631 MPa-m/sec18000 psi-ft/min100 fpm
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmASTM D257
Dielectric Strength 16.5 kV/mm420 kV/inMethod A (Short-Time); ASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 27.0 µm/m-°C15.0 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 216 °C420 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 216 °C420 °FUnannealed; ASTM D648
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Evonik VESTAMID® HTplus M1533 PA6T/X, GF30
Techmer ES Luriblend® PA6/6 GF30 TS1 BK 30% Glass Filled
Techmer ES Luriblend® PA6/6 GF30 TL15 UV 30% Glass Filled
Techmer ES Luriblend® PA6/6 GF30 TL15 BK 30% Glass Filled
Techmer ES Luriblend® PA6/6 GF30 IM TL15 30% Glass Filled

PTPC0785 / 136723

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.