MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AdvanSix Aegis® HFX High Barrier Nylon  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Description: Aegis® HFX is an oxygen scavenging polyamide composition formulated specifically for use in high performance packaging applications where high gas barrier is required. This product is useful in injection and extrusion molding applications. Aegis® HFX offers high oxygen barrier, even at high humidity, outstanding delamination resistance and whitening resistance, clarity and easy processing (particularly in the PET co-injection stretch blow molding process).

Former Honeywell product; AdvanSix is a spin-off of Honeywell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.14 g/cc1.14 g/ccASTM D1505
Bulk Density 0.730 g/cc0.0264 lb/in³ISO 60
Oxygen Transmission <= 0.000787 cc-mm/m²-24hr-atm<= 0.00200 cc-mil/100 in²-24hr-atm80% RH, 23°C, cast film
Melt Index of Compound  13 g/10 min
@Load 2.16 kg,
Temperature 260 °C
13 g/10 min
@Load 4.76 lb,
Temperature 500 °F
ISO 1133
 26 g/10 min
@Load 2.16 kg,
Temperature 280 °C
26 g/10 min
@Load 4.76 lb,
Temperature 536 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 51.4 MPa7450 psiISO 527
Tensile Strength, Yield 83.4 MPa12100 psiISO 527
Elongation at Break 192 %192 %ISO 527
Elongation at Yield 5.2 %5.2 %ISO 527
Flexural Strength 110 MPa16000 psiISO 178
Flexural Modulus 2.54 GPa368 ksiISO 178
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 72.5 °C163 °FISO 1133
Deflection Temperature at 1.8 MPa (264 psi) 66.8 °C152 °FISO 1133
Glass Transition Temp, Tg 82.0 °C180 °FDSC method
 
Processing PropertiesMetricEnglishComments
Processing Temperature 265 - 280 °C509 - 536 °FManifold
Feed Temperature 35.0 °C95.0 °F
Nozzle Temperature 265 °C509 °F
Zone 1 245 °C473 °F
Zone 2 265 °C509 °F
Zone 3 265 °C509 °F
Zone 4 265 °C509 °F
Zone 5 265 °C509 °F
 
Descriptive Properties
Melt Temperature Amorphous
Oxygen Scav. Capacitymin 10 cc/gGC Method

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Honeywell ACLAR® SupRx 900 CTFE Homopolymer, Barrier Film
DuPont Teijin Films Melinex® WCW Polyester Film, 75 Gauge
DuPont Teijin Films Melinex® 343 Polyester Film, 200 Gauge
AdvanSix Aegis® OX High Barrier Nylon
Petromont 2200 High Density Polyethylene Resin

PALA01 / 23093

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.