MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Delrin® 500MT NC010 POM-I  (discontinued **)
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Homopolymer, Unreinforced, Impact Grade

Material Notes: Medium Toughened, Toughened, Medium Viscosity Acetal Homopolymer

Information provided by DuPont; The Delrin product line was sold by DuPont in 2023 but this specific grade was discontinued prior to the sale

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ISO 1183
Water Absorption 1.9 %
@Thickness 2.00 mm
1.9 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.300 %
@Thickness 2.00 mm
0.300 %
@Thickness 0.0787 in
2mm; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.014 cm/cm0.014 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.015 cm/cm0.015 in/innormal; ISO 294-4, 2577
Melt Flow 9.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
9.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 43.0 MPa6240 psiISO 527-1/-2
Elongation at Break 42 %42 %Nominal; ISO 527-1/-2
Elongation at Yield 22 %22 %ISO 527-1/-2
Tensile Modulus 1.60 GPa232 ksiISO 527-1/-2
Flexural Modulus 1.50 GPa218 ksiISO 178
Poissons Ratio 0.420.42
Izod Impact, Notched (ISO)  9.00 kJ/m²
@Temperature -40.0 °C
4.28 ft-lb/in²
@Temperature -40.0 °F
ISO 180/1A
 16.0 kJ/m²
@Temperature 23.0 °C
7.61 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 2.00 J/cm²
@Temperature 23.0 °C
9.52 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 130 µm/m-°C72.2 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 130 µm/m-°C72.2 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 127 °C261 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 66.0 °C151 °FISO 75-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 20 %20 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 210 °C392 - 410 °FInjection
 205 °C401 °FOptimum, Injection
Mold Temperature 40.0 - 60.0 °C104 - 140 °FInjection
 50.0 °C122 °FOptimum, Injection
Drying Temperature 80.0 °C
@Time 14400 - 28800 sec
176 °F
@Time 4.00 - 8.00 hour
Injection; Dehumidified Dryer
Moisture Content 0.050 %0.050 %
Hold Pressure 60.0 - 80.0 MPa8700 - 11600 psiInjection
Annealing Temperature 160 °C320 °FOptional; 30 min/mm
 
Descriptive Properties
AdditivesRelease agent
Delivery formPellets
Drying Recommendedyes
FeaturesUltrasonic Weldable
FMVSS ClassBISO 3795 (FMVSS 302)
Hold pressure time (s/mm)7.5Injection
Part Marking Code>POM-I<ISO 11469
ProcessingExtrusion - small Tubing
 Extrusion - Wire and Cable
 Injection Molding
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPOM-IISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDSX5117f / 254328

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.