SABIC CYCOLAC™ DL100LG ABS (Americas)
Categories:
Polymer
;
Thermoplastic
;
ABS Polymer
Material Notes:
CYCOLAC DL100LG is a low gloss, high heat, high impact ABS/PC blend with low emission
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.08
g/cc
0.0390
lb/in³
ISO 1183
Linear Mold Shrinkage, Flow
0.0050
-
0.0070
cm/cm
0.0050
-
0.0070
in/in
SABIC method
Melt Flow
10
g/10 min
@Load 10.0 kg,
Temperature 220 °C
10
g/10 min
@Load 22.0 lb,
Temperature 428 °F
cm³/10 min; ISO 1133
10
g/10 min
@Load 10.0 kg,
Temperature 220 °C
10
g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
12
g/10 min
@Load 5.00 kg,
Temperature 260 °C
12
g/10 min
@Load 11.0 lb,
Temperature 500 °F
cm³/10 min; ISO 1133
Mechanical Properties
Metric
English
Comments
Ball Indentation Hardness
80.0
MPa
11600
psi
ISO 2039-1
Tensile Strength at Break
36.0
MPa
5220
psi
5 mm/min; ISO 527
38.0
MPa
5510
psi
50 mm/min; ASTM D638
39.0
MPa
5660
psi
50 mm/min; ISO 527
40.0
MPa
5800
psi
5 mm/min; ASTM D638
Tensile Strength, Yield
47.0
MPa
6820
psi
5 mm/min; ASTM D638
47.0
MPa
6820
psi
5 mm/min; ISO 527
51.0
MPa
7400
psi
50 mm/min; ISO 527
51.0
MPa
7400
psi
50 mm/min; ASTM D638
Elongation at Break
12 %
12 %
50 mm/min; ISO 527
12 %
12 %
50 mm/min; ASTM D638
50 %
50 %
5 mm/min; ISO 527
85 %
85 %
5 mm/min; ASTM D638
Elongation at Yield
4.0 %
4.0 %
5 mm/min; ASTM D638
4.0 %
4.0 %
50 mm/min; ISO 527
4.0 %
4.0 %
50 mm/min; ASTM D638
4.0 %
4.0 %
5 mm/min; ISO 527
Tensile Modulus
2.20
GPa
319
ksi
1mm/min; ISO 527
2.24
GPa
325
ksi
50 mm/min; ASTM D638
Flexural Yield Strength
74.0
MPa
10700
psi
2 mm/min; ISO 178
Flexural Modulus
2.20
GPa
319
ksi
2 mm/min; ISO 178
Izod Impact, Notched
3.80
J/cm
7.12
ft-lb/in
ASTM D256
1.15
J/cm
@Temperature -30.0 °C
2.15
ft-lb/in
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO)
28.0
kJ/m²
13.3
ft-lb/in²
80*10*4; ISO 180/1A
45.0
kJ/m²
21.4
ft-lb/in²
80*10*3; ISO 180/1A
11.0
kJ/m²
@Temperature -30.0 °C
5.23
ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
19.0
kJ/m²
@Temperature -30.0 °C
9.04
ft-lb/in²
@Temperature -22.0 °F
80*10*3; ISO 180/1A
Charpy Impact, Notched
2.20
J/cm²
10.5
ft-lb/in²
Edgew 80*10*3 sp=62mm; ISO 179/1eA
1.10
J/cm²
@Temperature -30.0 °C
5.23
ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
82.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
45.6
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow
83.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
46.1
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
103
°C
217
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi)
84.0
°C
183
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
85.0
°C
@Thickness 6.40 mm
185
°F
@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point
105
°C
221
°F
Rate B/50; ISO 306
107
°C
225
°F
Rate B/120; ISO 306
118
°C
244
°F
Rate A/50; ISO 306
120
°C
248
°F
Rate A/120; ISO 306
Processing Properties
Metric
English
Comments
Processing Temperature
60.0
-
80.0
°C
140
-
176
°F
Hopper Temperature
Nozzle Temperature
245
-
275
°C
473
-
527
°F
Injection Molding
Zone 1
230
-
260
°C
446
-
500
°F
Zone 2
250
-
280
°C
482
-
536
°F
Zone 3
250
-
280
°C
482
-
536
°F
Melt Temperature
250
-
280
°C
482
-
536
°F
Mold Temperature
40.0
-
80.0
°C
104
-
176
°F
Drying Temperature
90.0
-
100
°C
194
-
212
°F
Injection Molding
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Injection Molding
Moisture Content
0.10 %
0.10 %
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABI10006 / 243473
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.