MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC NORYL™ Resin SE1GFN3 Polyphenylene Ether + PS (PPE+PS) (Europe)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ SE1GFN3 resin is a 30% glass reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of V1 at 1.5mm along with UL746C Outdoor Suitability rating of F1 and RTI of 110C. NORYL SE1GFN3 exhibits high heat resistance, good dielectric strength, dimensional stability, hydrolytic stability, and very low moisture absorption. This material is an excellent candidate for a variety of applications such as solar frames, unattended power supply (UPS) inverter/charger, indoor and outdoor electrical enclosures / housings / connectors, and wall plates / sockets / switches.

Features: Hydrolytic Stability,Low Creep Sensitivity,Good Stiffness,Non-Halogenated,Non-Chlorinated,Non-Brominated,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.29 g/ccISO 1183
Moisture Absorption 0.0700 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.23 %ISO 62-1
Viscosity 9.0 cP
@Load 10.0 kg,
Temperature 280 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cmSABIC method
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 130 MPaH358/30; ISO 2039-1
Tensile Strength at Break 105 MPa5 mm/min; ISO 527
Elongation at Break 2.0 %5 mm/min; ISO 527
Tensile Modulus 8000 MPa1 mm/min; ISO 527
Flexural Strength 130 MPabreak, 2mm/min; ISO 178
Flexural Modulus 6000 MPa2 mm/min; ISO 178
Izod Impact, Unnotched (ISO) 25.0 kJ/m²80*10*4; ISO 180/1U
 25.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 30.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 30.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Taber Abrasion, mg/1000 Cycles 55CS-17, 1 kg; SABIC method
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.0
@Frequency 1e+6 Hz
IEC 60250
 3.1
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 16.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 25.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
 30.0 kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
IEC 60250
 0.0080
@Frequency 50.0 - 60.0 Hz
IEC 60250
Comparative Tracking Index 175 - 250 VUL 746A
 300 VIEC 60112
Hot Wire Ignition, HWI >= 120 sec
@Thickness >=1.50 mm
UL 746A
High Amp Arc Ignition, HAI 0.00 - 15 arcs
@Thickness >=1.50 mm
UL 746A
 15 - 30 arcs
@Thickness >=6.00 mm
UL 746A
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 30.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 37.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 37.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 55.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 55.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Thermal Conductivity 0.280 W/m-KISO 8302
Hot Ball Pressure Test 125 °CPASS; IEC 60695-10-2
 140 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 140 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 135 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 145 °CRate B/50; ISO 306
 150 °CRate B/120; ISO 306
 155 °CRate A/50; ISO 306
UL RTI, Electrical 110 °CUL 746B
UL RTI, Mechanical with Impact 105 °CUL 746B
UL RTI, Mechanical without Impact 110 °CUL 746B
Flammability, UL94 V-1
@Thickness >=1.50 mm
UL 94
 V-0
@Thickness >=6.00 mm
UL 94
 5VA
@Thickness >=3.00 mm
UL 94
Oxygen Index 31 %ISO 4589
Glow Wire Flammability Index 960 °C
@Thickness 3.20 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 280 - 300 °C
Zone 2 280 - 300 °C
Zone 3 300 - 320 °C
Melt Temperature 300 - 320 °CInjection Molding
Mold Temperature 100 - 130 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 2.00 - 3.00 hourInjection Molding
Precipitation Temperature 80.0 - 100 °CHopper Temperature
 
Descriptive Properties
UV-light, water exposure/immersionF2UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82473 / 290420

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.