MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Melos Mecoline S TP 1013 F Halogen-free, thermoplastic, flame retardant sheathing
Categories: Polymer; Thermoplastic

Material Notes: Halogen-free, thermoplastic, flame retardant sheathing compound for low and medium voltage cables

Compound class: Sheathing

Compound category: TP

Flame retardant: ATH

Standards: DIN EN 50363-8 TM7; DIN VDE 0276-604 HM4; DIN VDE 0281 part 14 TM7; IEC 60092-360 SHF 1; VDE 0207 part 24 HM2, HM4; VDE 0250 part 215 HM5

Typical applications: Halogen-free, low smoke, thermoplastic, highly oil and extra fuel resistant, flame retardant compound for the sheathing of low and medium voltage cables for moving applications. (e. g. Green Energy/Offshore)

Features: Flame retardant; Halogen-free; Low smoke; Flexible; Flexible at low temperatures: Low smoke; Oil resistant

Information provided by Melos

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.61 g/cc0.0582 lb/in³pressed plaques, 165°C / 5 min; DIN EN ISO 1183-1A
pH >= 5.0>= 5.0Corrosivity, Acid gas emission; IEC 60754-2
Mooney Viscosity 58
@Temperature 160 °C
58
@Temperature 320 °F
ML (1+4); DIN ISO 289-1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8989pressed plaques, 165°C / 5 min; DIN ISO 7619-1
Tensile Strength 10.8 MPa1570 psiextruded tapes; IEC 60811-501
 9.71 MPa
@Temperature 150 °C,
Time 360000 sec
1410 psi
@Temperature 302 °F,
Time 100 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 10.1 MPa
@Temperature 136 °C,
Time 605000 sec
1460 psi
@Temperature 277 °F,
Time 168 hour
extruded tapes, After ageing in air oven; IEC 60811-401
 11.502 MPa
@Temperature 90.0 °C,
Time 1.21e+6 sec
1668.2 psi
@Temperature 194 °F,
Time 336 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 11.804 MPa
@Temperature 100 °C,
Time 432000 sec
1712.0 psi
@Temperature 212 °F,
Time 120 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 12.204 MPa
@Temperature 80.0 °C,
Time 5.18e+6 sec
1770.0 psi
@Temperature 176 °F,
Time 1440 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 12.6 MPa
@Temperature 80.0 °C,
Time 605000 sec
1830 psi
@Temperature 176 °F,
Time 168 hour
extruded tapes, After ageing in air oven; IEC 60811-401
 99.82 MPa
@Temperature 23.0 °C,
Time 86400 sec
14480 psi
@Temperature 73.4 °F,
Time 24.0 hour
extruded tapes, Diesel; IEC 60811-404
 101.01 MPa
@Temperature 100 °C,
Time 86400 sec
14650 psi
@Temperature 212 °F,
Time 24.0 hour
extruded tapes, Diesel; IEC 60811-404
Elongation at Break 300 %300 %extruded tapes; IEC 60811-501
 235.8 %
@Temperature 100 °C,
Time 86400 sec
235.8 %
@Temperature 212 °F,
Time 24.0 hour
extruded tapes, Diesel; IEC 60811-404
 257.4 %
@Temperature 23.0 °C,
Time 86400 sec
257.4 %
@Temperature 73.4 °F,
Time 24.0 hour
extruded tapes, Diesel; IEC 60811-404
 267 %
@Temperature 136 °C,
Time 605000 sec
267 %
@Temperature 277 °F,
Time 168 hour
extruded tapes, After ageing in air oven; IEC 60811-401
 273 %
@Temperature 80.0 °C,
Time 605000 sec
273 %
@Temperature 176 °F,
Time 168 hour
extruded tapes, After ageing in air oven; IEC 60811-401
 285.9 %
@Temperature 100 °C,
Time 432000 sec
285.9 %
@Temperature 212 °F,
Time 120 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 291 %
@Temperature 90.0 °C,
Time 1.21e+6 sec
291 %
@Temperature 194 °F,
Time 336 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 312.9 %
@Temperature 80.0 °C,
Time 5.18e+6 sec
312.9 %
@Temperature 176 °F,
Time 1440 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
 411.3 %
@Temperature 150 °C,
Time 360000 sec
411.3 %
@Temperature 302 °F,
Time 100 hour
extruded tapes, Fluid IRM 902; IEC 60811-404
Penetration  12
@Temperature 90.0 °C,
Time 21600 sec
12
@Temperature 194 °F,
Time 6.00 hour
[%] Hot pressure test, extruded tapes; IEC 60811-508
 18
@Temperature 100 °C,
Time 21600 sec
18
@Temperature 212 °F,
Time 6.00 hour
[%] Hot pressure test, extruded tapes; IEC 60811-508
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity  3.80e+10 ohm-cm
@Temperature 90.0 °C
3.80e+10 ohm-cm
@Temperature 194 °F
500V; VDE 0303-30
 2.20e+11 ohm-cm
@Temperature 23.0 °C
2.20e+11 ohm-cm
@Temperature 73.4 °F
500V; VDE 0303-30
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 90.0 °C194 °F
Minimum Service Temperature, Air -50.0 °C-58.0 °F
Brittleness Temperature -42.0 °C-43.6 °FASTM D 746
 
Processing PropertiesMetricEnglishComments
Processing Temperature 70.0 - 180 °C158 - 356 °FMaximum mass temperature
 160 - 180 °C320 - 356 °FTool
Zone 1 130 - 150 °C266 - 302 °F
Zone 2 140 - 160 °C284 - 320 °F
Zone 3 140 - 160 °C284 - 320 °F
Zone 4 150 - 170 °C302 - 338 °F
Zone 5 150 - 170 °C302 - 338 °F
Adapter Temperature 155 - 175 °C311 - 347 °F
Head Temperature 160 - 180 °C320 - 356 °F
Drying Temperature 60.0 - 70.0 °C140 - 158 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour
Shelf Life 12.0 Month12.0 Month
 
Component Elements PropertiesMetricEnglishComments
Loss on Ignition(%) 38 %38 %pressed plaques, 165°C / 5 min.; ASTM D 2863 A
 
Descriptive Properties
Cold bend testNo cracksat -40°C, IEC 60811-504
Conductivity<0.4 µS/mmpressed plaques, 165°C / 5 min, IEC 60754-2
Main burning properties<5 mg/gAmount of halogen acid gas, IEC 60754-1
Pulley flexing test>30000 cyclesEN 50 396 cl. 6.2
Toxicity index<1.2NES 713
 3.6ITC, EN 50305

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PMELOS006 / 296113

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.