MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 3844 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 3844 is an 80 durometer black colored Buna N elastomer, it is formulated with FDA sanctioned materials. It exhibits good resistance to compression set, petroleum based oils, aliphatic and aromatic fuels.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 820 B14 B34 EO14 EO34; 3 BG 820 B14; 4 BG 820 B14 EO34; 6 BG 820 A14 B14 B34 EO14 EO34; 7 BG 820 B14 EA14 EF11 EF21 EO14 EO34; 3 CH 820 A25 B14 B34 EO16 EO36; 4 CH 820 A25 B14 B34 EO15 EO35 F14; 5 CH 820 B14 B34 EF31 EO36; 6 CH 820 B14 B34 EF31 EO36

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.27 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 82
 68
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 71
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 80
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 80
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 81
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 81
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
 81
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 85
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 86
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 87
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 87
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 91
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 94
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 2308 psi
 1901.8 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1991.8 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 2340.3 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 2421.1 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 2501.9 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 2515.7 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 2524.95 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 2541.1 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
 2548.03 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 2631.12 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 2663.4 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 2679.588 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Elongation, Ultimate 280 %
 168 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 201.1 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 205.2 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3
 206.1 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 220.1 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1
 231 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 236.88 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1
 241.92 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3
 264.1 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3
 281.12 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1
 290.92 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 407.1 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
100% Modulus 1139 psi
Tear Strength 242 pliDie C
 325 pliDie B
Compression Set 5.4 %
@Temperature 100 °C,
Time 79200 sec
Solid
 8.4 %
@Temperature 100 °C,
Time 252000 sec
Solid
 12.7 %
@Temperature 100 °C,
Time 79200 sec
Plied
 17.5 %
@Temperature 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Shrinkage -8.50 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -7.60 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -5.70 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -0.300 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.010 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 1.1 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #3
 2.4 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 3.3 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 18.4 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 30.6 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL030 / 318240

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.