MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC LNP™ THERMOCOMP™ Compound MX06402H Polypropylene, Unspecified (PP, Unspecified)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: LNP THERMOCOMP MX06402H compound is based on Polypropylene (PP) resin containing 20% glass fiber. Added features of this grade include: Heat Stabilized, Low Extractables, Healthcare.

Features: Low Extractable,Healthcare,High Stiffness,Heat Stabilized,Food Contact Acceptable,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.06 g/cc1.06 g/ccASTM D792
Density 1.05 g/cc0.0379 lb/in³ISO 1183
Moisture Absorption 0.0100 %0.0100 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0070 - 0.0090 cm/cm0.0070 - 0.0090 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.010 - 0.030 cm/cm0.010 - 0.030 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 34.0 MPa4930 psi5 mm/min; ASTM D638
 35.0 MPa5080 psi5 mm/min; ISO 527
Tensile Strength, Yield 37.0 MPa5370 psi5 mm/min; ISO 527
 38.0 MPa5510 psi5 mm/min; ASTM D638
Elongation at Break 2.7 %2.7 %5 mm/min; ISO 527
 3.4 %3.4 %5 mm/min; ASTM D638
Elongation at Yield 1.7 %1.7 %5 mm/min; ISO 527
 2.0 %2.0 %5 mm/min; ASTM D638
Tensile Modulus 5.35 GPa776 ksi1 mm/min; ISO 527
 6.39 GPa927 ksi50 mm/min; ASTM D638
Flexural Strength 65.0 MPa9430 psiISO 178
 66.0 MPa9570 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 4.69 GPa680 ksi2 mm/min; ISO 178
 4.70 GPa682 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 48.0 J35.4 ft-lbASTM D256
Izod Impact, Unnotched 1.95 J/cm3.65 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 4.00 kJ/m²1.90 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 13.0 kJ/m²6.19 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 12.0 J8.85 ft-lbASTM D3763
Impact Test 2.00 J1.48 ft-lbMultiaxial Impact; ISO 6603
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 45.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
25.0 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow 101 µm/m-°C
@Temperature -30.0 - 30.0 °C
56.1 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 134 °C273 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 143 °C
@Thickness 3.20 mm
289 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °C203 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 103 °C
@Thickness 3.20 mm
217 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 215 - 225 °C419 - 437 °F
Zone 3 240 - 250 °C464 - 482 °F
Melt Temperature 225 - 250 °C437 - 482 °FInjection Molding
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Drying Temperature 80.0 °C176 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81731 / 289678

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.