SABIC LEXAN™ Copolymer SLX2071T Polycarbonate (PC)
Categories:
Polymer
;
Thermoplastic
;
Polycarbonate (PC)
Material Notes:
High viscosity PC copolymer blend with enhanced UV stabilization and added release agent. V2 rated. Available in transparent and tinted colors
Features: Weatherable
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.20
g/cc
1.20
g/cc
ASTM D792
Density
1.20
g/cc
0.0434
lb/in³
ISO 1183
Moisture Absorption
0.150 %
0.150 %
23°C / 50% RH; ISO 62
Water Absorption at Saturation
0.35 %
0.35 %
ISO 62-1
Viscosity
5.0
cP
@Load 1.20 kg,
Temperature 300 °C
5.0
cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow
0.0050
-
0.0070
cm/cm
@Thickness 3.20 mm
0.0050
-
0.0070
in/in
@Thickness 0.126 in
SABIC method
Melt Flow
6.0
g/10 min
@Load 1.20 kg,
Temperature 300 °C
6.0
g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
76.0
MPa
11000
psi
50 mm/min; ASTM D638
76.0
MPa
11000
psi
50 mm/min; ISO 527
Tensile Strength, Yield
67.0
MPa
9720
psi
50 mm/min; ASTM D638
67.0
MPa
9720
psi
50 mm/min; ISO 527
Elongation at Break
>= 100 %
>= 100 %
50 mm/min; ASTM D638
>= 100 %
>= 100 %
50 mm/min; ISO 527
Elongation at Yield
6.3 %
6.3 %
50 mm/min; ASTM D638
6.3 %
6.3 %
50 mm/min; ISO 527
Tensile Modulus
2.34
GPa
339
ksi
5 mm/min; ASTM D638
2.34
GPa
339
ksi
1 mm/min; ISO 527
Flexural Strength
96.0
MPa
13900
psi
yld, 1.3 mm/min, 50 mm span; ASTM D790
96.0
MPa
13900
psi
yield, 2 mm/min; ISO 178
Flexural Modulus
2.12
GPa
307
ksi
1.3 mm/min, 50 mm span; ASTM D790
2.12
GPa
307
ksi
2 mm/min; ISO 178
Izod Impact Notched
820
J
605
ft-lb
ASTM D256
140
J
@Temperature -30.0 °C
103
ft-lb
@Temperature -22.0 °F
ASTM D256
Dart Drop, Total Energy
85.0
J
62.7
ft-lb
ASTM D3763
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
70.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
70.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow
70.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
70.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi)
121
°C
250
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
134
°C
@Thickness 3.20 mm
273
°F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point
135
°C
275
°F
Rate B/50; ASTM D1525
137
°C
279
°F
Rate B/50; ISO 306
139
°C
282
°F
Rate B/120; ISO 306
Optical Properties
Metric
English
Comments
Haze
0.50 %
@Thickness 2.54 mm
0.50 %
@Thickness 0.100 in
ASTM D1003
Transmission, Visible
89 %
@Thickness 2.54 mm
89 %
@Thickness 0.100 in
ASTM D1003
Processing Properties
Metric
English
Comments
Processing Temperature
60.0
-
100
°C
140
-
212
°F
Calibrator Temperature
Zone 1
240
-
280
°C
464
-
536
°F
Profile Extrusion
Zone 2
240
-
280
°C
464
-
536
°F
Profile Extrusion
Zone 3
220
-
240
°C
428
-
464
°F
Profile Extrusion
Zone 4
220
-
240
°C
428
-
464
°F
Profile Extrusion
Adapter Temperature
220
-
240
°C
428
-
464
°F
Profile Extrusion
Die Temperature
245
-
290
°C
473
-
554
°F
Profile Extrusion
Melt Temperature
220
-
250
°C
428
-
482
°F
Profile Extrusion
Drying Temperature
105
°C
221
°F
Profile Extrusion
Dry Time
2.00
-
3.00
hour
2.00
-
3.00
hour
Profile Extrusion
Precipitation Temperature
60.0
-
80.0
°C
140
-
176
°F
Hopper Temperature
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH80420 / 288367
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.