MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI E 52100 Steel (100Cr6, SUJ2, UNS G52986)
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 5000 Series Steel; Low Alloy Steel; Carbon Steel; High Carbon Steel

Material Notes: E52100 has metallurgical and processing characteristics similar to alloy TBS-9.

Key Words: UNI 100 Cr 6 (Ital.), B.S. 534 A 99, B.S. 535 A 99, ASTM A 295, ASTM A295, ASTM A519, ASTM A535, ASTM A646, ASTM A711, MIL SPEC MIL-S-980, MIL SPEC MIL-S-7420, MIL SPEC MIL-S-22141, SAE J404, SAE J412, SAE J770, DIN 1.3505, AFNOR 100 C 6(Fr), 100Cr6, UNS G52986, AMS 6440, AMS 6441, AMS 6444, AMS 6447, ASTM A322, ASTM A331, ASTM A505; SUJ2
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.81 g/cc0.282 lb/in³annealed
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 55
@Temperature 593 °C
55
@Temperature 1100 °F
Hardness, Rockwell C 6262quenched in oil from 150°C tempered. (after 1 hour at tempering temperature)
 6464quenched in water from 150°C tempered. (after 1 hour at tempering temperature)
 6464quenched in oil
 6666quenched in water
 11
@Temperature 471 °C
11
@Temperature 880 °F
 20
@Temperature 427 °C
20
@Temperature 800 °F
 42
@Temperature 316 °C
42
@Temperature 600 °F
 53
@Temperature 204 °C
53
@Temperature 400 °F
 59
@Temperature 93.3 °C
59
@Temperature 200 °F
 61
@Temperature -17.8 °C
61
@Temperature 0.000 °F
Hardness, Vickers  100
@Temperature 588 °C
100
@Temperature 1090 °F
 140
@Temperature 538 °C
140
@Temperature 1000 °F
 250
@Temperature 427 °C
250
@Temperature 800 °F
 420
@Temperature 316 °C
420
@Temperature 600 °F
 580
@Temperature 204 °C
580
@Temperature 400 °F
 690
@Temperature 93.3 °C
690
@Temperature 200 °F
 710
@Temperature -17.8 °C
710
@Temperature 0.000 °F
Modulus of Elasticity 210 GPa30500 ksi
Bulk Modulus 160 GPa23200 ksiTypical for steels.
Poissons Ratio 0.300.30Calculated
Fracture Toughness 15.4 - 18.7 MPa-m½14.0 - 17.0 ksi-in½cracks originating in case; case depth 0.30 to 0.35 in.
Machinability 40 %40 %spheroidized annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPa11600 ksiTypical for steel
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000219 ohm-cm0.0000219 ohm-cmTypical 5000 series steel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.9 µm/m-°C
@Temperature 23.0 - 280 °C
6.61 µin/in-°F
@Temperature 73.4 - 536 °F
annealed
 12.5 µm/m-°C
@Temperature 23.0 - 280 °C
6.94 µin/in-°F
@Temperature 73.4 - 536 °F
hardened
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical 5000 series steel
Thermal Conductivity 46.6 W/m-K323 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.98 - 1.1 %0.98 - 1.1 %
Chromium, Cr 1.3 - 1.6 %1.3 - 1.6 %
Iron, Fe 96.5 - 97.32 %96.5 - 97.32 %As remainder
Manganese, Mn 0.25 - 0.45 %0.25 - 0.45 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.15 - 0.30 %0.15 - 0.30 %
Sulfur, S <= 0.025 %<= 0.025 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Crucible Steel AISI 52100 Alloy Steel
Latrobe Lescalloy® 52100 VAC-ARC High Performance Bearing Steel
AISI 1018 Steel, cold drawn
AISI 4140 Steel, normalized at 870°C (1600°F), air cooled, 13 mm (0.5 in.) round
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900

M521AA / 8220

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.