Calcium Hydroxyapatite, Ca10(PO4)6(OH)2
Categories: Ceramic; Oxide; Wood and Natural Products

Material Notes: Calcium hydroxyapatite is a natural constituent of teeth and bone, along with other calcium-phosphate ceramic (CPC) materials. Synthetic hydroxyapatite is used as an active bioceramic for teeth and bone replacement. Ionic substitution is common and plays a large role in the structure and properties of hydroxyapatites.

Key Words: Ca10(PO4)6(OH)2
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 3.05 - 3.15 g/cc0.110 - 0.114 lb/in³
 3.219 g/cc0.1163 lb/in³Calculated (for zero porosity)
Porosity 0.10 - 3.0 %0.10 - 3.0 %
a Lattice Constant 9.432 Å9.432 Å
c Lattice Constant 6.881 Å6.881 Å
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 38.0 - 48.0 MPa5510 - 6960 psi
Modulus of Elasticity 7.00 - 13.0 GPa1020 - 1890 ksi
Flexural Strength 100 - 120 MPa14500 - 17400 psi
Compressive Strength 350 - 450 MPa50800 - 65300 psi
Poissons Ratio 0.270.27
Shear Modulus 2.76 - 5.12 GPa400 - 743 ksiCalculated
 
Descriptive Properties
Unit CellHexagonal

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.