MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 3741 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 3741 is a 70 durometer black colored Buna N elastomer, it is formulated with FDA sanctioned materials. It is also suitable for use in milk and edible oils.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 715 B14 B34 EO14 EO34; 2 BG 715 B14 B34 EO14 EO34 EA14 EF11 EF21; 5 BG 715 A14 B14 B34 EO14 EO34; 4 BK 715 A24 B14 B34 EF11 EO14 EO34; 2 CH 715 A25 B14 B34 EO15 EO35 EF31; 3 CH 715 A25 B14 B34 EO16 EO36
3-A Sanitary Standards 18-03 Class lll & lV
CFR 21 177.2600

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.23 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 73
 58
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 60
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 67
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 68
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 68
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 68
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 72
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 74
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 75
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 75
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 76
@Temperature 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 76
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 82
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 82
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 87
@Temperature 150 °C,
Time 252000 sec
Heat Aged
Tensile Strength 1510 psi
 697.6 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 768.6 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 945.3 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 1040.4 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 1556.8 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 1632.3 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 1632.3 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1695.7 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1736.5 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 1763.7 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 1763.7 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1825.6 psi
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 1866.4 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 1955.5 psi
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
Elongation, Ultimate 425 %
 54.8 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 251.2 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 299.2 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 314.9 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 376.1 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 393.1 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 393.1 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 402.05 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 402.05 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 445.8 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 447.9 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 462.8 %
@Temperature 100 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 478.97 %
@Temperature 125 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 486.2 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
100% Modulus 386 psi
Tear Strength 182 pliDie B
 233 pliDie C
Compression Set 7.3 %
@Temperature 100 °C,
Time 79200 sec
Solid
 10.3 %
@Temperature 125 °C,
Time 79200 sec
Solid
 11.8 %
@Temperature 100 °C,
Time 252000 sec
Solid
 13.7 %
@Temperature 100 °C,
Time 79200 sec
Plied
 17.3 %
@Temperature 125 °C,
Time 79200 sec
Plied
 24.9 %
@Temperature 150 °C,
Time 79200 sec
Solid
 31.3 %
@Temperature 150 °C,
Time 79200 sec
Plied
 50.5 %
@Temperature 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -8.00 °F
Shrinkage -5.40 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #1 (IRM 901)
 -5.30 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1 (IRM 901)
 -5.00 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #1 (IRM 901)
 1.9 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 3.6 %
@Temperature 100 °C,
Time 252000 sec
Volume, ASTM Oil #3 (IRM 903)
 4.3 %
@Temperature 125 °C,
Time 252000 sec
Volume, ASTM Oil #3 (IRM 903)
 5.5 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3 (IRM 903)
 10.9 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 25.1 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 42 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack
TR-10 Temperature-24°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL021 / 318231

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.