MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Chase Plastics CP Pryme® PC100RUL-18M BK Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: 18 Melt Prime Polycarbonate, Black Pellets.

Information provided by Chase Plastics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccASTM D792
Water Absorption 0.15 %
@Time 86400 sec
ASTM D570
Moisture Absorption at Equilibrium 0.35 %
@Temperature 22.8 °C
ASTM D570
 0.58 %
@Temperature 100 °C
ASTM D570
Melt Flow 18 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 70ASTM D785
Hardness, Rockwell R 118ASTM D785
Tensile Strength at Break 10000 psiType I, 2.0 in/min.; ASTM D638
Tensile Strength, Yield 9000 psiType I, 2.0 in/min.; ASTM D638
Elongation at Break 130 %Type I, 2.0 in/min.; ASTM D638
Elongation at Yield 7.0 %Type I, 2.0 in/min.; ASTM D638
Flexural Yield Strength 14000 psi0.051 in/min. 1.97 inch span; ASTM D790
Flexural Modulus 340000 psi0.051 in/min. 1.97 inch span; ASTM D790
Izod Impact, Notched 13.0 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Izod Impact, Unnotched 60.0 ft-lb/in
@Temperature 22.8 °C
ASTM D256
Izod Impact, Notched (ISO) 5.20 ft-lb/in²
@Temperature -30.0 °C
80*10*3.; ISO 180/1A
 31.0 ft-lb/in²
@Temperature 22.8 °C
80*10*3.; ISO 180/1A
Izod Impact, Unnotched (ISO) NB
@Temperature -30.0 °C
80*10*3.; ISO 180/1U
 NB
@Temperature 22.8 °C
80*10*3.; ISO 180/1U
Charpy Impact Unnotched NB
@Temperature -30.0 °C
80*10*3 sp=62mm.; ISO 179/1eU
 NB
@Temperature 22.8 °C
80*10*3 sp=62mm.; ISO 179/1eU
Charpy Impact, Notched 5.70 ft-lb/in²
@Temperature -30.0 °C
80*10*3 sp=62mm.; ISO 179/1eA
 31.0 ft-lb/in²
@Temperature 22.8 °C
80*10*3 sp=62mm.; ISO 179/1eA
Gardner Impact 1500 in-lb
@Temperature 22.8 °C
ASTM D3029
Tensile Impact Strength 260 ft-lb/in²Type S.; ASTM D1822
Dart Drop, Total Energy 45.8 ft-lb
@Temperature 22.8 °C
ASTM D3763
Taber Abrasion, mg/1000 Cycles 101000 g, CS-17 Wheel.; ASTM D1044
 
Thermal PropertiesOriginal ValueComments
CTE, linear 38.0 µin/in-°F
@Temperature -40.0 - 95.0 °C
ASTM E831
Specific Heat Capacity 0.300 BTU/lb-°FASTM C351
Thermal Conductivity 1.70 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 280 °F
@Thickness 6.40 mm
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 265 °F
@Thickness 6.40 mm
Unannealed; ASTM D648
Vicat Softening Point 310 °FRate B (120°C/h), Loading 2 (50 N).; ASTM D1525
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.586ASTM D542
Haze 1.0 %
@Thickness 2.54 mm
ASTM D1003
UV Transmittance 88 %
@Thickness 2.54 mm
ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCHA938 / 268589

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.