MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Copper Alloy, UNS C26130, OS015 Temper, Flat Products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Nominal Grain Size 0.015 mm

Fabrication Properties: Excellent Suitability – Soldering, Brazing, Capacity for Being Cold Worked; Good Suitability – Oxyacetylene Welding, Spot Weld, Butt Weld; Fair Suitability – Gas Shielded Arc Welding, Capacity for Being Hot Formed

Typical Uses: Grillwork; Auto Radiator Tube; Heater Cord; Radiators; Tanks; Finish Hardware; Hinges; Kick Plates; Locks; Push Plates; Stencils; Flashlight Shells; Lamp Fixtures; Reflectors; Screw Shells; Eyelets; Fasteners; Grommets; Pins; Rivets; Screws; Bead Chain; Chain; Liners; Power Cylinders; Pumps; Springs; Ammunition Components; Plumbing Accessories; Plumbing Brass Goods

Applicable Specifications: Tube: Heat Exchanger – B569

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.53 g/cc0.308 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell F 7878
Hardness, Rockwell 30T 4343
Tensile Strength 365 MPa53000 psi
Tensile Strength, Yield 152 MPa22000 psi0.5% Ext
Elongation at Break 54 %54 %
Tensile Modulus 110 GPa16000 ksi
Modulus of Rigidity 41.4 GPa6000 ksi
Poissons Ratio 0.330.33Calculated
Fatigue Strength 96.5 MPa
@# of Cycles 1.00e+8
14000 psi
@# of Cycles 1.00e+8
Shear Strength 241 MPa35000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000610 ohm-cm0.00000610 ohm-cm28% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.0 µm/m-°C
@Temperature 20.0 - 300 °C
11.1 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 10.1 W/m-K70.0 BTU-in/hr-ft²-°F
Melting Point 916 - 954 °C1680 - 1750 °F
Solidus 916 °C1680 °F
Liquidus 954 °C1750 °F
Annealing Point 427 - 760 °C800 - 1400 °F
 
Processing PropertiesMetricEnglishComments
Hot-Working Temperature 732 - 843 °C1350 - 1550 °F
 
Component Elements PropertiesMetricEnglishComments
Arsenic, As 0.020 - 0.080 %0.020 - 0.080 %
Copper, Cu 68.5 - 71.5 %68.5 - 71.5 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.050 %<= 0.050 %
Zinc, Zn 28.4 - 31.5 %28.4 - 31.5 %As Balance
 
Descriptive Properties
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC26130x6 / 291791

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.