MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ COLORCOMP™ Compound D1000FL Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP COLORCOMP D1000FL compound is based on unfilled Polycarbonate (PC) resin. Added features of this grade include: Superior Molding, Low Extractable.

Features: Low Extractable,Aesthetics and Appearance,Superior Molding,Custom Color,Food Contact Acceptable

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.300 %0.300 %23°C/50% RH/24 hrs; ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 64.0 MPa9280 psi5 mm/min; ASTM D638
Elongation at Yield 6.0 %6.0 %5 mm/min; ASTM D638
Tensile Modulus 2.39 GPa347 ksi50 mm/min; ASTM D638
 
Electrical PropertiesMetricEnglishComments
Arc Resistance 0.00 - 60 sec0.00 - 60 secASTM D495
Comparative Tracking Index >= 600 V>= 600 VUL 746A
Hot Wire Ignition, HWI  30 - 60 sec
@Thickness >=1.50 mm
30 - 60 sec
@Thickness >=0.0591 in
UL 746A
 60 - 120 sec
@Thickness >=6.00 mm
60 - 120 sec
@Thickness >=0.236 in
UL 746A
High Amp Arc Ignition, HAI  30 - 60 arcs
@Thickness >=1.50 mm
30 - 60 arcs
@Thickness >=0.0591 in
UL 746A
 60 - 120 arcs
@Thickness >=3.00 mm
60 - 120 arcs
@Thickness >=0.118 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR 0.000 - 10.0 mm/min0.000 - 0.394 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.170 W/m-K1.18 BTU-in/hr-ft²-°FASTM E1530
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
UL RTI, Electrical 125 °C257 °FUL 746B
UL RTI, Mechanical with Impact 115 °C239 °FUL 746B
UL RTI, Mechanical without Impact 125 °C257 °FUL 746B
Flammability, UL94  HB
@Thickness >=2.70 mm
HB
@Thickness >=0.106 in
UL 94
 V-2
@Thickness >=1.00 mm
V-2
@Thickness >=0.0394 in
UL 94
 
Processing PropertiesMetricEnglishComments
Zone 2 310 - 320 °C590 - 608 °F
Zone 3 320 - 330 °C608 - 626 °F
Melt Temperature 305 - 325 °C581 - 617 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80533 / 288480

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.