MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC LNP™ STAT-KON™ Compound ME006 Polypropylene, Unspecified (PP, Unspecified) (Americas)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: LNP STAT-KON ME006 compound is based on Polypropylene (PP) resin containing 30% carbon fiber. Added features of this grade include: Electrically Conductive.

Features: High Stiffness,Light-weight Structural,Super Strong (Carbon Fiber Filled),Electrically Conductive

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 g/cc0.0383 lb/in³ASTM D792
 1.06 g/cc0.0383 lb/in³ISO 1183
Moisture Absorption 0.0300 %0.0300 %23°C/50% RH/24 hrs; ASTM D570
 0.0300 %0.0300 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0020 - 0.0040 cm/cm0.0020 - 0.0040 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0070 - 0.0090 cm/cm0.0070 - 0.0090 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.0 MPa7980 psi5 mm/min; ISO 527
 57.0 MPa8270 psi5 mm/min; ASTM D638
Tensile Strength, Yield 56.0 MPa8120 psi5 mm/min; ISO 527
 58.0 MPa8410 psi5 mm/min; ASTM D638
Elongation at Break 0.50 %0.50 %5 mm/min; ASTM D638
 0.50 %0.50 %5 mm/min; ISO 527
Elongation at Yield 0.50 %0.50 %5 mm/min; ASTM D638
 0.50 %0.50 %5 mm/min; ISO 527
Tensile Modulus 13.99 GPa2029 ksi1 mm/min; ISO 527
 17.34 GPa2515 ksi50 mm/min; ASTM D638
Flexural Strength 58.0 MPa8410 psiISO 178
 78.0 MPa11300 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 12.3 GPa1780 ksi1.3 mm/min, 50 mm span; ASTM D790
 12.33 GPa1788 ksi2 mm/min; ISO 178
Izod Impact Notched 41.0 J30.2 ft-lbASTM D256
Izod Impact, Unnotched 0.820 J/cm1.54 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 4.00 kJ/m²1.90 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 4.00 kJ/m²1.90 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 10.0 J7.38 ft-lbASTM D3763
Impact Test 3.00 J2.21 ft-lbMultiaxial Impact; ISO 6603
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 10 - 1000 ohm10 - 1000 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 23.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
12.8 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow 59.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
32.8 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 153 °C307 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 153 °C
@Thickness 3.20 mm
307 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 132 °C
@Thickness 3.20 mm
270 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 215 - 225 °C419 - 437 °F
Zone 3 240 - 250 °C464 - 482 °F
Melt Temperature 225 - 250 °C437 - 482 °FInjection Molding
Mold Temperature 30.0 - 50.0 °C86.0 - 122 °F
Drying Temperature 80.0 °C176 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81320 / 289267

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.