MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

SABIC ULTEM™ Resin AUT200M Polyetherimide (PEI)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: High flow Polyetherimide (Tg 217C) with internal mold release.. Very low outgassing and plateout, for automotive lighting applications where highly metallized, reflective surfaces are required. Haze onset temperature of 204C (SABIC IP method).

Features: High Stiffness,Hydrolytic Stability,Chemical Resistance,Low Smoke and Toxicity,Good Mechanicals in Broad Temperature Range,Low Creep Sensitivity,Low Shrinkage,Good metal adhesion,Amorphous,High Strength,High Heat Resistance,Good dimensional stability,Flame Retardant,Good Mold Release

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.27 g/cc0.0459 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.700 %0.700 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 1.25 %1.25 %ISO 62-1
Viscosity 13 cP
@Load 5.00 kg,
Temperature 340 °C
13 cP
@Load 11.0 lb,
Temperature 644 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inSABIC method
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 140 MPa20300 psiH358/30; ISO 2039-1
Tensile Strength at Break 85.0 MPa12300 psi50 mm/min; ISO 527
Tensile Strength, Yield 105 MPa15200 psi50 mm/min; ISO 527
Elongation at Break 60 %60 %50 mm/min; ISO 527
Elongation at Yield 6.0 %6.0 %50 mm/min; ISO 527
Tensile Modulus 3.30 GPa479 ksi1 mm/min; ISO 527
Flexural Strength 160 MPa23200 psiyield, 2 mm/min; ISO 178
Flexural Modulus 3.30 GPa479 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*4; ISO 180/1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
80*10*4; ISO 180/1U
Taber Abrasion, mg/1000 Cycles 1010CS-17, 1 kg; SABIC method
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 50.0 µm/m-°C
@Temperature 23.0 - 150 °C
27.8 µin/in-°F
@Temperature 73.4 - 302 °F
ISO 11359-2
CTE, linear, Transverse to Flow 50.0 µm/m-°C
@Temperature 23.0 - 150 °C
27.8 µin/in-°F
@Temperature 73.4 - 302 °F
ISO 11359-2
Thermal Conductivity 0.240 W/m-K1.67 BTU-in/hr-ft²-°FISO 8302
Deflection Temperature at 0.46 MPa (66 psi) 195 °C383 °FEdgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 190 °C374 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 211 °C412 °FRate B/50; ISO 306
 212 °C414 °FRate B/120; ISO 306
 215 °C419 °FRate A/50; ISO 306
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 350 - 405 °C662 - 761 °F
Zone 2 350 - 405 °C662 - 761 °F
Zone 3 360 - 415 °C680 - 779 °F
Melt Temperature 370 - 410 °C698 - 770 °FInjection Molding
Mold Temperature 140 - 180 °C284 - 356 °F
Drying Temperature 150 °C302 °FInjection Molding
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection Molding
Precipitation Temperature 80.0 - 120 °C176 - 248 °FHopper Temperature
 
Descriptive Properties
Metallized Haze Onset204 °CSABIC method

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82669 / 290616

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.