MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC LNP™ LUBRICOMP™ Compound KCL34A Acetal (POM) Homopolymer
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: LNP LUBRICOMP KCL34A compound is based on Acetal (POM) Homopolymer resin containing 15% PTFE, 20% carbon fiber. Added features of this grade include: Wear Resistant, Electrically Conductive.

Features: Light-weight Structural,Super Strong (Carbon Fiber Filled),Wear resistant,Electrically Conductive,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.55 g/cc0.0560 lb/in³ISO 1183
 1.56 g/cc0.0564 lb/in³ASTM D792
Moisture Absorption 0.300 %0.300 %23°C/50% RH/24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0070 cm/cm0.0070 in/in24hrs; ASTM D955
 0.0073 cm/cm0.0073 in/in24hrs; ISO 294
Linear Mold Shrinkage, Transverse 0.013 cm/cm0.013 in/in24hrs; ASTM D955
 0.013 cm/cm0.013 in/in24hrs; ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 87.0 MPa12600 psiASTM D638
 88.0 MPa12800 psiISO 527
Tensile Strength, Yield 87.0 MPa12600 psiASTM D638
 88.0 MPa12800 psiISO 527
Elongation at Break 0.70 %0.70 %ASTM D638
 0.70 %0.70 %ISO 527
Elongation at Yield 0.70 %0.70 %ASTM D638
 0.70 %0.70 %ISO 527
Tensile Modulus 15.51 GPa2250 ksi1 mm/min; ISO 527
 17.23 GPa2499 ksi50 mm/min; ASTM D638
Flexural Strength 110 MPa16000 psiASTM D790
 117 MPa17000 psiISO 178
Flexural Modulus 13.1 GPa1900 ksiASTM D790
 15.0 GPa2180 ksiISO 178
Izod Impact Notched 53.0 J39.1 ft-lbASTM D256
Izod Impact, Unnotched 2.67 J/cm5.00 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 3.00 kJ/m²1.43 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 16.0 kJ/m²7.61 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 4.00 J2.95 ft-lbpeak; ASTM D3763
Impact Test 1.00 J0.738 ft-lbMultiaxial Impact; ISO 6603
Coefficient of Friction, Dynamic 0.350.35ASTM D3702 Modified: Manual
Coefficient of Friction, Static 0.320.32ASTM D3702 Modified: Manual
K (wear) Factor 139 x 10-8 mm³/N-M69.0 x 10-10 in³-min/ft-lb-hrWasher; ASTM D3702 Modified: Manual
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1.00e+6 ohm1.00e+6 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  27.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
15.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 27.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
15.0 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  66.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
36.7 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 66.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
37.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 175 °C347 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 175 °C
@Thickness 3.20 mm
347 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 170 °C338 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 171 °C
@Thickness 3.20 mm
340 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 195 - 205 °C383 - 401 °F
Zone 3 210 - 220 °C410 - 428 °F
Melt Temperature 200 - 215 °C392 - 419 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 80.0 °C176 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80824 / 288771

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.