MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Ajedium™ Film - AvaSpire® AV-630 Polyaryletherketone (PAEK)
Categories: Polymer; Film; Thermoplastic; Polyketone; Polyaryletherketone (PAEK), Unreinforced

Material Notes: Similar to the high strength and chemical resistance of PEEK, but with higher ductility.

AvaSpire® AV-630 PAEK film is a unique thermoplastic film that is characterized by a distinct combination of properties, which include strength, ductility, fatigue resistance, high purity and excellent chemical resistance to organics, acids, and bases. These properties make it well-suited for applications in aerospace, electronics, transportation, chemical processing, and other industrial uses.

Applications: Aircraft Applications; Automotive Applications; Electrical/Electronic Applications; Industrial Applications; Medical/Healthcare Applications; Oil/Gas Applications

Features: Chemical Resistant; Ductile; Fatigue Resistant; Flame Retardant; Good Dimensional Stability; Good Impact Resistance; Good Sterilizability; High Heat Resistance; Radiation (Gamma) Resistant

Standard Thicknesses and Widths
- Widths are available from 22" (559 mm) to 56" (1422 mm). Products with widths <22 inches or >56 inches are available upon request.
- Tolerances for widths are +/- 4mm.
- For PAEK film, the standard thicknesses are 12 microns (0.5 mil) to 1016 microns (40 mil).

Surface Finishes
- Standard surface finish is P/M (polished / matte).
- Custom finishes of P/P (polished / polished) and M/M (matte / matte) are available.

Packaging
- Film is supplied in a roll form of high quality, cardboard core of 3" (76mm) or 6" (152mm).
- PVC cores are available upon request in 3" and 6" sizes.

Labeling
- Products are labeled to comply with national and international standards.
- Labels include product grade, unique batch number, roll length, roll width, product thickness, and net weight.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccASTM D792
Water Absorption 0.20 %
@Time 86400 sec
ASTM D570
Thickness 50.0 micronsAs Tested
 100 micronsAs Tested
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 71.7 MPaASTM D882
Film Tensile Strength at Yield, TD 68.9 MPaASTM D882
Film Elongation at Break, MD 130 %ASTM D882
Film Elongation at Break, TD 130 %ASTM D882
Film Elongation at Yield, MD 5.0 %ASTM D882
Film Elongation at Yield, TD 5.0 %ASTM D882
Secant Modulus, MD 2.04 GPaASTM D882
Secant Modulus, TD 2.00 GPaASTM D882
Dart Drop Test 830 gASTM D1709
Film Tensile Strength at Break, MD 86.9 MPaASTM D882
Film Tensile Strength at Break, TD 83.4 MPaASTM D882
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.60e+14 ohm-cmASTM D257
Surface Resistance >= 1.90e+17 ohmASTM D257
Dielectric Constant 3.05
@Frequency 1e+6 Hz
ASTM D150
 3.06
@Frequency 60 Hz
ASTM D150
 3.1
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 200 kV/mm
@Thickness 0.0500 mm
ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 43.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
ASTM E831
Thermal Conductivity 0.240 W/m-KASTM C177
Melting Point 340 °CPeak; ASTM D3418
Glass Transition Temp, Tg 158 °CDSC
Oxygen Index 38 %ASTM D2863
 
Descriptive Properties
Area Factor149 ft²/lb/mil
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorTranslucent
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4001 / 279801

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.