SABIC CYCOLOY™ MC1300 PC+ABS (Americas)
Categories:
Polymer
;
Thermoplastic
;
ABS Polymer
;
Polycarbonate/ABS Alloy, Unreinforced
Material Notes:
PC/ABS, excellent flow and impact performance, plating and painting applications.
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.10
g/cc
1.10
g/cc
ASTM D792
Water Absorption
0.10 %
0.10 %
24 hours; ASTM D570
Linear Mold Shrinkage, Flow
0.0050
-
0.0080
cm/cm
@Thickness 3.20 mm
0.0050
-
0.0080
in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse
0.0050
-
0.0070
cm/cm
@Thickness 3.20 mm
0.0050
-
0.0070
in/in
@Thickness 0.126 in
SABIC method
Melt Flow
14
g/10 min
@Load 5.00 kg,
Temperature 260 °C
14
g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
44.0
MPa
6380
psi
50 mm/min; ASTM D638
Tensile Strength, Yield
50.0
MPa
7250
psi
50 mm/min; ASTM D638
Elongation at Break
150 %
150 %
50 mm/min; ASTM D638
Elongation at Yield
8.6 %
8.6 %
50 mm/min; ASTM D638
Tensile Modulus
2.13
GPa
309
ksi
50 mm/min; ASTM D638
Flexural Yield Strength
72.0
MPa
10400
psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus
2.10
GPa
305
ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched
5.34
J/cm
10.0
ft-lb/in
ASTM D256
4.27
J/cm
@Temperature -30.0 °C
8.00
ft-lb/in
@Temperature -22.0 °F
ASTM D256
Dart Drop, Total Energy
41.0
J
30.2
ft-lb
ASTM D3763
33.0
J
@Temperature -30.0 °C
24.3
ft-lb
@Temperature -22.0 °F
ASTM D3763
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
72.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
40.0
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow
90.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
50.0
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Thermal Conductivity
0.200
W/m-K
1.39
BTU-in/hr-ft²-°F
ASTM C177
Deflection Temperature at 0.46 MPa (66 psi)
115
°C
@Thickness 3.20 mm
239
°F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
99.0
°C
@Thickness 3.20 mm
210
°F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point
112
°C
234
°F
Rate B/50; ASTM D1525
Processing Properties
Metric
English
Comments
Nozzle Temperature
260
-
290
°C
500
-
554
°F
Injection Molding
Zone 1
250
-
280
°C
482
-
536
°F
Zone 2
255
-
290
°C
491
-
554
°F
Zone 3
255
-
290
°C
491
-
554
°F
Melt Temperature
260
-
290
°C
500
-
554
°F
Mold Temperature
75.0
-
100
°C
167
-
212
°F
Drying Temperature
100
-
105
°C
212
-
221
°F
Injection Molding
Dry Time
3.00
-
4.00
hour
3.00
-
4.00
hour
Injection Molding
8.00
hour
8.00
hour
Cumulative; Injection Molding
Moisture Content
0.020 %
0.020 %
Back Pressure
0.300
-
0.700
MPa
43.5
-
102
psi
Shot Size
30 - 80 %
30 - 80 %
Vent Depth
0.00380
-
0.00760
cm
0.00150
-
0.00299
in
Screw Speed
40
-
70
rpm
40
-
70
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABI10757 / 244224
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.