MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Copolymer EXL1162T PC+Siloxane (Europe)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Siloxane

Material Notes: LEXAN EXL1162T polycarbonate (PC) siloxane copolymer resin is a transparent injection molding (IM) grade with extra release properties. This resin offers good low temperature (-20 C) ductility in combination with high flow characteristics and excellent processability with opportunities for shorter IM cycle times compared to standard PC resins. LEXAN EXL1162T resin is a general purpose product available in transparent and opaque colors and may be an excellent candidate for a broad range of applications.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Density 1.19 g/ccISO 1183
Water Absorption 0.12 %23°C/sat; ISO 62
Moisture Absorption 0.0900 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 19 g/10 min
@Load 1.20 kg,
Temperature 300 °C
cm³/10 min; ISO 1133
 20 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell L 89ISO 2039-2
Tensile Strength at Break 56.0 MPa50 mm/min; ISO 527
 57.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 57.0 MPa50 mm/min; ISO 527
 58.0 MPa50 mm/min; ASTM D638
Elongation at Break 117.9 %50 mm/min; ASTM D638
 119.4 %50 mm/min; ISO 527
Elongation at Yield 5.4 %50 mm/min; ISO 527
 5.7 %50 mm/min; ASTM D638
Tensile Modulus 2260 MPa50 mm/min; ASTM D638
 2340 MPa1mm/min; ISO 527
Flexural Yield Strength 89.0 MPa2 mm/min; ISO 178
 94.0 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2140 MPa2 mm/min; ISO 178
 2240 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 736 J/mASTM D256
 618 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 55.0 kJ/m²80*10*3; ISO 180/1A
 40.0 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*3; ISO 180/1U
 NB
@Temperature -30.0 °C
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 65.0 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 45.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 74.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmASTM D257
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 74.8 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 74.8 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
CTE, linear, Transverse to Flow 76.4 µm/m-°C
@Temperature -40.0 - 95.0 °C
ASTM E831
 76.4 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Hot Ball Pressure Test 125 °CIEC 60695-10-2
Deflection Temperature at 1.8 MPa (264 psi) 116 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 121 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 138 °CRate A/50; ASTM D1525
 138 °CRate B/50; ISO 306
 139 °CRate B/120; ISO 306
 
Optical PropertiesOriginal ValueComments
Haze 3.0 %
@Thickness 2.54 mm
ASTM D1003
Transmission, Visible 82 %
@Thickness 2.54 mm
ASTM D1003
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °CInjection Molding
Zone 1 270 - 295 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °C
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI11821 / 245288

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.