Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
SABIC LNP™ THERMOCOMP™ Compound WX15003 Polybutylene Terephthalate (PBT)
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), Unreinforced, Molded
Material Notes:
LNP THERMOCOMP WX15003 compound is based on Polybutylene Terephthalate (PBT) resin containing 45 % glass fiber/mineral. Added features of this grade include: UV stabilized.
Features: UV Resistant,Low Warpage,Structural
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.83
g/cc
ISO 1183
Moisture Absorption
0.0200 %
Injection Molding
Viscosity
11
cP
@Load 1.20 kg,
Temperature 265 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow
0.0020
-
0.0060
cm/cm
SABIC method
Mechanical Properties
Original Value
Comments
Ball Indentation Hardness
145
MPa
H358/30; ISO 2039-1
Tensile Strength at Break
100
MPa
5 mm/min; ISO 527
Elongation at Break
2.0 %
5 mm/min; ISO 527
Tensile Modulus
8000
MPa
1 mm/min; ISO 527
Flexural Strength
140
MPa
break, 2mm/min; ISO 178
Flexural Modulus
7400
MPa
2 mm/min; ISO 178
Izod Impact, Notched (ISO)
5.00
kJ/m²
80*10*4; ISO 180/1A
4.00
kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
33.0
kJ/m²
80*10*4; ISO 180/1U
31.0
kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched
35.0
kJ/m²
Edgew 80*10*4 sp=62mm; ISO 179/1eU
35.0
kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched
4.00
kJ/m²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
3.00
kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Taber Abrasion, mg/1000 Cycles
76
CS-17, 1 kg; SABIC method
Electrical Properties
Original Value
Comments
Volume Resistivity
>=
1.00e+15
ohm-cm
IEC 60093
Surface Resistance
>=
1.00e+15
ohm
ROA; IEC 60093
Dielectric Constant
3.5
@Frequency 1e+6 Hz
IEC 60250
3.6
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dissipation Factor
0.0010
@Frequency 50.0 - 60.0 Hz
IEC 60250
0.013
@Frequency 1e+6 Hz
IEC 60250
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
25.0
µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
30.0
µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow
75.0
µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
80.0
µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Thermal Conductivity
0.330
W/m-K
ISO 8302
Hot Ball Pressure Test
125
°C
PASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi)
220
°C
Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)
180
°C
Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point
200
°C
Rate B/120; ISO 306
200
°C
Rate B/50; ISO 306
220
°C
Rate A/50; ISO 306
Glow Wire Flammability Index
750
°C
@Thickness 3.20 mm
IEC 60695-2-12
Processing Properties
Original Value
Comments
Nozzle Temperature
245
-
270
°C
Zone 2
240
-
260
°C
Zone 3
250
-
270
°C
Melt Temperature
255
-
280
°C
Injection Molding
Mold Temperature
60.0
-
100
°C
Drying Temperature
110
-
120
°C
Injection Molding
Dry Time
2.00
-
4.00
hour
Injection Molding
Precipitation Temperature
40.0
-
60.0
°C
Hopper Temperature
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PSABH81965 / 289912
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.