MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC CYCOLOY™ MC8100 PC+ABS (Americas)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: PC/ABS, extrusion and blow molding grade.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.13 g/cc1.13 g/ccASTM D792
Water Absorption 0.10 %0.10 %24 hours; ASTM D570
Moisture Absorption at Equilibrium 0.40 %0.40 %ASTM D570
Linear Mold Shrinkage, Flow 0.0040 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0040 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 52.0 MPa7540 psi50 mm/min; ASTM D638
Elongation at Break 100 %100 %50 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %50 mm/min; ASTM D638
Tensile Modulus 2.06 GPa299 ksi50 mm/min; ASTM D638
Flexural Yield Strength 77.0 MPa11200 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.06 GPa299 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 5.34 J/cm10.0 ft-lb/inASTM D256
 4.27 J/cm
@Temperature -30.0 °C
8.00 ft-lb/in
@Temperature -22.0 °F
ASTM D256
Dart Drop, Total Energy 54.0 J39.8 ft-lbASTM D3763
 47.0 J
@Temperature -30.0 °C
34.7 ft-lb
@Temperature -22.0 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 81.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
45.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 123 °C
@Thickness 3.20 mm
253 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 104 °C
@Thickness 3.20 mm
219 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Zone 1 240 - 250 °C464 - 482 °FExtrusion Blow Molding
Zone 2 240 - 255 °C464 - 491 °FExtrusion Blow Molding
Zone 3 240 - 255 °C464 - 491 °FExtrusion Blow Molding
Zone 4 240 - 255 °C464 - 491 °FExtrusion Blow Molding
Zone 5 245 - 260 °C473 - 500 °F
Die Temperature 250 - 265 °C482 - 509 °FExtrusion Blow Molding
Melt Temperature 245 - 260 °C473 - 500 °F
Head Temperature 245 - 260 °C473 - 500 °FZone 6 - Top Temperature
 245 - 260 °C473 - 500 °FZone 7 - Bottom Temperature
Mold Temperature 40.0 - 90.0 °C104 - 194 °F
Drying Temperature 100 - 110 °C212 - 230 °FExtrusion Blow Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourExtrusion Blow Molding
 24.0 hour24.0 hourCumulative; Extrusion Blow Molding
Moisture Content >= 0.040 %>= 0.040 %
 0.040 - 0.050 %0.040 - 0.050 %
Screw Speed 20 - 50 rpm20 - 50 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI10763 / 244230

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.