MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Copper, UNS C62400 (Aluminum Bronze 11%), M30 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Temper: As Hot Extruded

Fabrication Properties: Excellent Suitability – Capacity for Being Hot Formed; Good Suitability – Gas Shielded Arc Welding, Coated Metal Arc Welding, Spot Weld, Seam Weld, Butt Weld; Fair Suitability – Brazing; Poor Suitability – Capacity for Being Cold Worked

Common Fabrication Processes: Hot bending; Hot forging

Typical uses: Nuts; Bushings; Cams; Drift Pins; Gears; Hydraulic Bushings; Support Bushings; Tie Rods; Valve Balls; Wear Plates; Welding Wire

Applicable Specifications: Forgings – SAE J461, SAE J463; Rod – Welding AWS A5.7; Rod, Bar & Shapes - Aluminum Bronze ASTM B150/B150M, Aluminum Bronze ASME SB150

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.269 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 87
@Thickness 102 mm
Tensile Strength 90.0 ksi
@Thickness 102 mm
Tensile Strength, Yield 40.0 ksi
@Thickness 102 mm
0.5% Ext
Elongation at Break 18 %
@Thickness 102 mm
Tensile Modulus 17000 ksi
Modulus of Rigidity 6400 ksi
Poissons Ratio 0.33Calculated
Fatigue Strength 32000 psi
@Thickness 102 mm,
# of Cycles 1.00e+8
Machinability 50 %
Forgeability 80 %
Shear Strength 58.0 ksi
@Thickness 102 mm
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000143 ohm-cm12% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.00 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 34.0 BTU-in/hr-ft²-°F
Melting Point 1880 - 1900 °F
Solidus 1880 °F
Liquidus 1900 °F
Annealing Point 1100 - 1200 °F
 
Processing PropertiesOriginal ValueComments
Hot-Working Temperature 1400 - 1625 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 10 - 11.5 %
Copper, Cu 83.3 - 88 %As Balance
Iron, Fe 2.0 - 4.5 %
Manganese, Mn <= 0.30 %
Silicon, Si <= 0.25 %
Tin, Sn <= 0.20 %
 
Descriptive Properties
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC62400x4 / 293040

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.