MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
EOS NickelAlloy IN939 DMSL on EOS M 290
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Nonferrous Metal; Lead Alloy

Material Notes: EOS NickelAlloy IN939 is a nickel-chromium alloy which provides an outstanding balance of high temperature strength, corrosion and oxidation resistance, fatigue performance and creep strength at temperatures up to 850 °C (1 560 °F). Parts built from EOS NickelAlloy IN939 can be hardened after manufacture by application of precipitation- hardening heat treatments.

Main Characteristics:

  • Excellent corrosion and oxidation resistance
  • High tensile, fatigue, creep and rupture strength at temperatures up to 850 °C (1 560 °F)
  • Maintains good ductility in age-hardened condition
  • Crack-free in as-built condition and resistant to strain-age cracking
Typical Applications:
  • Industrial gas turbines (vanes, blades, heat-shields)
  • Microturbines
  • Turbochargers
  • Instrumentation parts
  • Power industry parts
  • Process industry parts

Information provided by EOS GmbH (Electro Optical Systems).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.15 g/ccISO 3369
Particle Size 20 - 55 µm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 33As-Manufactured; ISO 6508
 48Heat Treated; ISO 6508
Tensile Strength, Ultimate >= 1090 MPaVertical, as manufactured; ISO 6892-1
 >= 1160 MPaHorizontal, as manufactured; ISO 6892-1
 >= 300 MPa
@Temperature 950 °C
Vertical, heat treated; ISO 6892-2
 >= 310 MPa
@Temperature 950 °C
Horizontal, heat treated; ISO 6892-2
 >= 400 MPa
@Temperature 900 °C
Vertical, heat treated; ISO 6892-2
 >= 410 MPa
@Temperature 900 °C
Horizontal, heat treated; ISO 6892-2
 >= 550 MPa
@Temperature 850 °C
Horizontal, heat treated; ISO 6892-2
 >= 600 MPa
@Temperature 850 °C
Vertical, heat treated; ISO 6892-2
 >= 750 MPa
@Temperature 800 °C
Horizontal, heat treated; ISO 6892-2
 >= 770 MPa
@Temperature 800 °C
Vertical, heat treated; ISO 6892-2
 >= 900 MPa
@Temperature 750 °C
Vertical, heat treated; ISO 6892-2
 >= 900 MPa
@Temperature 750 °C
Horizontal, heat treated; ISO 6892-2
 >= 1050 MPa
@Temperature 700 °C
Vertical, heat treated; ISO 6892-2
 >= 1050 MPa
@Temperature 700 °C
Horizontal, heat treated; ISO 6892-2
 >= 1380 MPa
@Temperature 600 °C
Vertical, heat treated; ISO 6892-2
 >= 1400 MPa
@Temperature 600 °C
Horizontal, heat treated; ISO 6892-2
 >= 1410 MPa
@Temperature 400 °C
Vertical, heat treated; ISO 6892-2
 >= 1430 MPa
@Temperature 400 °C
Horizontal, heat treated; ISO 6892-2
 >= 1500 MPa
@Temperature 23.0 °C
Vertical, heat treated; ISO 6892-1
 >= 1520 MPa
@Temperature 23.0 °C
Horizontal, heat treated; ISO 6892-1
Tensile Strength, Yield 740 MPaVertical, as manufactured; ISO 6892-1
 880 MPaHorizontal, as manufactured; ISO 6892-1
 200 MPa
@Temperature 950 °C
Horizontal, heat treated; ISO 6892-2
 210 MPa
@Temperature 950 °C
Vertical, heat treated; ISO 6892-2
 300 MPa
@Temperature 900 °C
Horizontal, heat treated; ISO 6892-2
 375 MPa
@Temperature 900 °C
Vertical, heat treated; ISO 6892-2
 430 MPa
@Temperature 850 °C
Horizontal, heat treated; ISO 6892-2
 500 MPa
@Temperature 850 °C
Vertical, heat treated; ISO 6892-2
 605 MPa
@Temperature 800 °C
Horizontal, heat treated; ISO 6892-2
 620 MPa
@Temperature 800 °C
Vertical, heat treated; ISO 6892-2
 760 MPa
@Temperature 750 °C
Horizontal, heat treated; ISO 6892-2
 795 MPa
@Temperature 750 °C
Vertical, heat treated; ISO 6892-2
 880 MPa
@Temperature 700 °C
Horizontal, heat treated; ISO 6892-2
 900 MPa
@Temperature 700 °C
Vertical, heat treated; ISO 6892-2
 990 MPa
@Temperature 600 °C
Vertical, heat treated; ISO 6892-2
 1000 MPa
@Temperature 600 °C
Horizontal, heat treated; ISO 6892-2
 1010 MPa
@Temperature 400 °C
Vertical, heat treated; ISO 6892-2
 1050 MPa
@Temperature 400 °C
Horizontal, heat treated; ISO 6892-2
 1100 MPa
@Temperature 23.0 °C
Vertical, heat treated; ISO 6892-1
 1130 MPa
@Temperature 23.0 °C
Horizontal, heat treated; ISO 6892-1
Elongation at Break 24 %Horizontal, as manufactured; ISO 6892-1
 28 %Vertical, as manufactured; ISO 6892-1
 1.75 %
@Temperature 800 °C
Horizontal, heat treated; ISO 6892-2
 2.0 %
@Temperature 700 °C
Horizontal, heat treated; ISO 6892-2
 2.5 %
@Temperature 750 °C
Horizontal, heat treated; ISO 6892-2
 2.5 %
@Temperature 850 °C
Horizontal, heat treated; ISO 6892-2
 5.0 %
@Temperature 900 °C
Horizontal, heat treated; ISO 6892-2
 5.0 %
@Temperature 800 °C
Vertical, heat treated; ISO 6892-2
 6.5 %
@Temperature 750 °C
Vertical, heat treated; ISO 6892-2
 7.0 %
@Temperature 850 °C
Vertical, heat treated; ISO 6892-2
 8.5 %
@Temperature 900 °C
Vertical, heat treated; ISO 6892-2
 8.5 %
@Temperature 950 °C
Horizontal, heat treated; ISO 6892-2
 9.5 %
@Temperature 600 °C
Horizontal, heat treated; ISO 6892-2
 9.5 %
@Temperature 700 °C
Vertical, heat treated; ISO 6892-2
 11 %
@Temperature 23.0 °C
Horizontal, heat treated; ISO 6892-1
 12.5 %
@Temperature 400 °C
Horizontal, heat treated; ISO 6892-2
 13 %
@Temperature 23.0 °C
Vertical, heat treated; ISO 6892-1
 13 %
@Temperature 400 °C
Vertical, heat treated; ISO 6892-2
 13.5 %
@Temperature 600 °C
Vertical, heat treated; ISO 6892-2
 20 %
@Temperature 950 °C
Vertical, heat treated; ISO 6892-2
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.79 µm/m-°C
@Temperature 25.0 - 100 °C
Heat Treated; ASTM E228
 12.18 µm/m-°C
@Temperature 25.0 - 100 °C
As Manufactured; ASTM E228
 12.64 µm/m-°C
@Temperature 25.0 - 200 °C
Heat Treated; ASTM E228
 12.89 µm/m-°C
@Temperature 25.0 - 200 °C
As Manufactured; ASTM E228
 13.49 µm/m-°C
@Temperature 25.0 - 600 °C
As Manufactured; ASTM E228
 13.64 µm/m-°C
@Temperature 25.0 - 400 °C
Heat Treated; ASTM E228
 13.78 µm/m-°C
@Temperature 25.0 - 400 °C
As Manufactured; ASTM E228
 13.99 µm/m-°C
@Temperature 25.0 - 800 °C
As Manufactured; ASTM E228
 14.27 µm/m-°C
@Temperature 25.0 - 600 °C
Heat Treated; ASTM E228
 15.06 µm/m-°C
@Temperature 25.0 - 900 °C
As Manufactured; ASTM E228
 15.29 µm/m-°C
@Temperature 25.0 - 800 °C
Heat Treated; ASTM E228
 16.32 µm/m-°C
@Temperature 25.0 - 900 °C
Heat Treated; ASTM E228
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 1.9 %
Boron, B 0.010 %
Carbon, C 0.15 %
Chromium, Cr 22.5 %
Cobalt, Co 19 %
Nickel, Ni 48.24 %Balance
Niobium, Nb (Columbium, Cb) 1.0 %
Tantalum, Ta 1.4 %
Titanium, Ti 3.7 %
Tungsten, W 2.0 %
Zirconium, Zr 0.10 %
 
Descriptive Properties
Volume rate3.6 mm3/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

NEOS935 / 280595

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.