MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECARAN ABS natural Acrylonitrile-butadiene-styrene copolymer
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes:
  • electrically insulating
  • high stiffness
  • good chemical resistance
  • low density
  • good damping
  • high toughness
  • low moisture absorption
Target Industries:
  • food processing
  • home appliances
  • automotive industry
  • fixture construction
  • food engineering
  • electronics
  • medical technology

Information provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.02 g/cc0.0368 lb/in³
Moisture Absorption 0.700 %0.700 %saturation; ASTM D570
 0.130 %
@Time 86400 sec
0.130 %
@Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 108108ASTM D785
Hardness, Shore D 7878ASTM D2240
Tensile Strength at Break 27.6 MPa4000 psiASTM D638
Tensile Strength, Yield 40.0 MPa5800 psiASTM D638
Elongation at Break 30 %30 %ASTM D638
Elongation at Yield 2.0 %2.0 %ASTM D638
Modulus of Elasticity 2.76 GPa400 ksiASTM D638
Flexural Strength 61.4 MPa8900 psiASTM D790
Flexural Modulus 2.14 GPa310 ksiASTM D790
Compressive Yield Strength 49.0 MPa
@Strain 10 %
7100 psi
@Strain 10 %
ASTM D695
Compressive Strength 22.1 MPa
@Strain 1 %
3200 psi
@Strain 1 %
ASTM D695
Compressive Modulus 2.59 GPa375 ksiASTM D695
Izod Impact, Notched 2.83 J/cm5.30 ft-lb/inASTM D256
Coefficient of Friction, Dynamic 0.35
@Pressure 0.276 MPa
0.35
@Pressure 40.0 psi
50 fpm; ASTM D3702
Coefficient of Friction, Static 0.19 - 0.210.19 - 0.21ASTM D3702
K (wear) Factor 7050 x 10-8 mm³/N-M3500 x 10-10 in³-min/ft-lb-hrAgainst Steel, 40 psi, 50 fpm; ASTM D 3702
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D257
Surface Resistivity per Square 1.00e+14 ohm1.00e+14 ohmASTM D257
Dielectric Constant 3.3
@Frequency 60 Hz
3.3
@Frequency 60 Hz
ASTM D150
Dielectric Strength 17.7 kV/mm450 kV/inASTM D149
Dissipation Factor 0.020
@Frequency 60 Hz
0.020
@Frequency 60 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 101 µm/m-°C
@Temperature -40.0 - 37.8 °C
56.0 µin/in-°F
@Temperature -40.0 - 100 °F
ASTM D696
Maximum Service Temperature, Air 71.1 °C160 °FLong Term
 98.9 °C210 °FIntermittent
Deflection Temperature at 0.46 MPa (66 psi) 93.3 °C200 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 80.6 °C177 °FASTM D648
Vicat Softening Point 107 °C224 °F
Glass Transition Temp, Tg 104 °C220 °FASTM D3418
Flammability, UL94 HBHB
 
Descriptive Properties
Colorbeige opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENSIN8199 / 319127

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.