MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC LNP™ COLORCOMP™ Compound EX12304C Polyetherimide (PEI)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: LNP COLORCOMP EX12304C compound is based on unfilled Polyetherimide (PEI) resin. Added features of this grade include: LNP Clean Compounding Technology.

Features: Aesthetics and Appearance,LNP Clean Compound Technology,Custom Color

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.27 g/ccASTM D792
Density 1.27 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
Viscosity 25 cP
@Load 5.00 kg,
Temperature 220 °C
MVR cc/10 min; ISO 1133
Melt Flow 17.8 g/10 min
@Load 6.60 kg,
Temperature 337 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 85.0 MPa5 mm/min; ISO 527
 105 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 105 MPa5 mm/min; ISO 527
 110 MPa5 mm/min; ASTM D638
Elongation at Break 60 %5 mm/min; ASTM D638
 60 %5 mm/min; ISO 527
Elongation at Yield 6.0 %5 mm/min; ISO 527
 7.0 %5 mm/min; ASTM D638
Tensile Modulus 3200 MPa1 mm/min; ISO 527
 3580 MPa5 mm/min; ASTM D638
Flexural Strength 160 MPayield, 2 mm/min; ISO 178
 174 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3300 MPa2 mm/min; ISO 178
 3420 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 32.0 JASTM D256
Izod Impact, Unnotched 1335 J/mASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 55.8 µm/m-°C
@Temperature -20.0 - 150 °C
ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 193 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 198 °C
@Thickness 6.40 mm
unannealed; ASTM D648
Vicat Softening Point 212 °CRate B/120; ISO 306
UL RTI, Electrical 105 °CUL 746B
UL RTI, Mechanical with Impact 105 °CUL 746B
UL RTI, Mechanical without Impact 105 °CUL 746B
Flammability, UL94 V-2
@Thickness >=0.750 mm
UL 94
 V-0
@Thickness >=3.00 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 390 - 400 °C
Zone 2 370 - 390 °C
Zone 3 380 - 400 °C
Melt Temperature 360 - 400 °CInjection Molding
Mold Temperature 140 - 180 °C
Drying Temperature 150 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
Back Pressure 0.300 - 0.700 MPa
Vent Depth 0.00250 - 0.00760 cm
 
Descriptive Properties
Screw speed (Circumferential speed)0.2-0.3 m/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80554 / 288501

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.