Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 3.51 g/cc | 3.51 g/cc |
|
Chemical Properties | Metric | English | Comments |
---|
Acid Class, SR | 51 | 51 |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Knoop | 420 @Load 0.0999 kg | 420 @Load 0.220 lb |
Modulus of Elasticity | 84.0 GPa | 12200 ksi |
Modulus of Rigidity | 32.7 GPa | 4740 ksi |
Poissons Ratio | 0.285 | 0.285 |
Abrasion | 313 | 313 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 8.80 µm/m-°C @Temperature -30.0 - 70.0 °C | 4.89 µin/in-°F @Temperature -22.0 - 158 °F |
| 10.3 µm/m-°C @Temperature 100 - 300 °C | 5.72 µin/in-°F @Temperature 212 - 572 °F |
Thermal Conductivity | 0.738 W/m-K @Temperature 35.0 °C | 5.12 BTU-in/hr-ft²-°F @Temperature 95.0 °F |
Transformation Temperature, Tg | 577 °C | 1070 °F |
Softening Point | 650 °C | 1200 °F |
Annealing Point | 559 °C | 1040 °F |
Strain Point | 539 °C | 1000 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.58996 @Wavelength 2325.42 nm | 1.58996 @Wavelength 2325.42 nm |
| 1.59514 @Wavelength 1970.09 nm | 1.59514 @Wavelength 1970.09 nm |
| 1.60064 @Wavelength 1529.58 nm | 1.60064 @Wavelength 1529.58 nm |
| 1.60545 @Wavelength 1128.64 nm | 1.60545 @Wavelength 1128.64 nm |
| 1.60703 @Wavelength 1013.98 nm | 1.60703 @Wavelength 1013.98 nm |
| 1.60977 @Wavelength 852.11 nm | 1.60977 @Wavelength 852.11 nm |
| 1.61164 @Wavelength 768.19 nm | 1.61164 @Wavelength 768.19 nm |
| 1.61334 @Wavelength 706.52 nm | 1.61334 @Wavelength 706.52 nm |
| 1.61503 @Wavelength 656.27 nm | 1.61503 @Wavelength 656.27 nm |
| 1.6155 @Wavelength 643.85 nm | 1.6155 @Wavelength 643.85 nm |
| 1.61594 @Wavelength 632.8 nm | 1.61594 @Wavelength 632.8 nm |
| 1.61791 @Wavelength 589.29 nm | 1.61791 @Wavelength 589.29 nm |
| 1.618 @Wavelength 587.56 nm | 1.618 @Wavelength 587.56 nm |
| 1.62033 @Wavelength 546.07 nm | 1.62033 @Wavelength 546.07 nm |
| 1.62479 @Wavelength 486.13 nm | 1.62479 @Wavelength 486.13 nm |
| 1.62534 @Wavelength 479.99 nm | 1.62534 @Wavelength 479.99 nm |
| 1.62938 @Wavelength 441.57 nm | 1.62938 @Wavelength 441.57 nm |
| 1.63008 @Wavelength 435.835 nm | 1.63008 @Wavelength 435.835 nm |
| 1.63448 @Wavelength 404.656 nm | 1.63448 @Wavelength 404.656 nm |
| 1.64195 @Wavelength 365.015 nm | 1.64195 @Wavelength 365.015 nm |
Abbe Number | 63.02 | 63.02 |
| 63.32 | 63.32 |
Optical Dispersion | 0.002971 | 0.002971 |
| 0.003394 | 0.003394 |
| 0.00439 | 0.00439 |
| 0.004826 | 0.004826 |
| 0.005017 | 0.005017 |
| 0.005296 | 0.005296 |
| 0.005298 | 0.005298 |
| 0.007997 | 0.007997 |
| 0.008469 | 0.008469 |
| 0.00976 | 0.00976 |
| 0.009843 | 0.009843 |
| 0.011862 | 0.011862 |
| 0.012085 | 0.012085 |
| 0.016603 | 0.016603 |
Transmission, Visible | 96.1 % @Thickness 10.0 mm, Wavelength 380 nm | 96.1 % @Thickness 0.394 in, Wavelength 380 nm |
| 97.8 % @Thickness 10.0 mm, Wavelength 390 nm | 97.8 % @Thickness 0.394 in, Wavelength 390 nm |
| 98.6 % @Thickness 10.0 mm, Wavelength 400 nm | 98.6 % @Thickness 0.394 in, Wavelength 400 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 420 nm | 99.1 % @Thickness 0.394 in, Wavelength 420 nm |
| 99.2 % @Thickness 10.0 mm, Wavelength 440 nm | 99.2 % @Thickness 0.394 in, Wavelength 440 nm |
| 99.4 % @Thickness 10.0 mm, Wavelength 460 nm | 99.4 % @Thickness 0.394 in, Wavelength 460 nm |
| 99.6 % @Thickness 10.0 mm, Wavelength 480 nm | 99.6 % @Thickness 0.394 in, Wavelength 480 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 500 nm | 99.7 % @Thickness 0.394 in, Wavelength 500 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 650 nm | 99.7 % @Thickness 0.394 in, Wavelength 650 nm |
| 99.7 % @Thickness 10.0 mm, Wavelength 700 nm | 99.7 % @Thickness 0.394 in, Wavelength 700 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 550 nm | 99.8 % @Thickness 0.394 in, Wavelength 550 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 600 nm | 99.8 % @Thickness 0.394 in, Wavelength 600 nm |
IR Transmittance | 85 % @Thickness 10.0 mm, Wavelength 2400 nm | 85 % @Thickness 0.394 in, Wavelength 2400 nm |
| 90 % @Thickness 10.0 mm, Wavelength 2200 nm | 90 % @Thickness 0.394 in, Wavelength 2200 nm |
| 96 % @Thickness 10.0 mm, Wavelength 2000 nm | 96 % @Thickness 0.394 in, Wavelength 2000 nm |
| 97.8 % @Thickness 10.0 mm, Wavelength 1800 nm | 97.8 % @Thickness 0.394 in, Wavelength 1800 nm |
| 99.1 % @Thickness 10.0 mm, Wavelength 1600 nm | 99.1 % @Thickness 0.394 in, Wavelength 1600 nm |
| 99.5 % @Thickness 10.0 mm, Wavelength 1400 nm | 99.5 % @Thickness 0.394 in, Wavelength 1400 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 800 nm | 99.8 % @Thickness 0.394 in, Wavelength 800 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 900 nm | 99.8 % @Thickness 0.394 in, Wavelength 900 nm |
| 99.8 % @Thickness 10.0 mm, Wavelength 1000 nm | 99.8 % @Thickness 0.394 in, Wavelength 1000 nm |
| 99.9 % @Thickness 10.0 mm, Wavelength 1200 nm | 99.9 % @Thickness 0.394 in, Wavelength 1200 nm |
UV Transmittance | 2.0 % @Thickness 10.0 mm, Wavelength 320 nm | 2.0 % @Thickness 0.394 in, Wavelength 320 nm |
| 17 % @Thickness 10.0 mm, Wavelength 330 nm | 17 % @Thickness 0.394 in, Wavelength 330 nm |
| 44 % @Thickness 10.0 mm, Wavelength 340 nm | 44 % @Thickness 0.394 in, Wavelength 340 nm |
| 69 % @Thickness 10.0 mm, Wavelength 350 nm | 69 % @Thickness 0.394 in, Wavelength 350 nm |
| 85 % @Thickness 10.0 mm, Wavelength 360 nm | 85 % @Thickness 0.394 in, Wavelength 360 nm |
| 92.4 % @Thickness 10.0 mm, Wavelength 370 nm | 92.4 % @Thickness 0.394 in, Wavelength 370 nm |
|
Descriptive Properties |
---|
Acid Resistance, Powder Method, RA(P) | 3 |
CCI | 0.00 B |
| 0.31 G |
| 0.31 R |
coloring, λ 5 | 325 |
coloring, λ 80 | 365 |
Coloring, Internal Transmission λ 0.05 | 322 |
Coloring, Internal Transmission λ 0.80 | 357 |
Knoop Hardness Class | 4 |
Ohara Code d | 618633 |
Ohara Code e | 620630 |
Phosphate Resistance, PR | 4 |
Photoelastic Constant (ß) | 1.41 |
Water Resistance, RW(P) | 1 |
Weathering Resistance (Surface Method) W(S)max | 1 |
Yield Point, At (°C) | 614 |