MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Pressure Seal 19234 Silicone
Categories: Polymer; Thermoset; Silicone

Material Notes: Compound 19234 is a 20 durometer salmon colored Silicone elastomer.

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.06 g/cc1.06 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 2020
 18
@Temperature 150 °C,
Time 252000 sec
18
@Temperature 302 °F,
Time 70.0 hour
ASTM Oil #1
 22
@Temperature 100 °C,
Time 252000 sec
22
@Temperature 212 °F,
Time 70.0 hour
Distilled water aged
 23
@Temperature 150 °C,
Time 252000 sec
23
@Temperature 302 °F,
Time 70.0 hour
Heat Aged
Tensile Strength 2.78 MPa403 psi
 2.453 MPa
@Temperature 150 °C,
Time 252000 sec
355.8 psi
@Temperature 302 °F,
Time 70.0 hour
Heat Aged
 2.559 MPa
@Temperature 150 °C,
Time 252000 sec
371.2 psi
@Temperature 302 °F,
Time 70.0 hour
ASTM Oil #1
Elongation, Ultimate 714 %714 %
 674 %
@Temperature 150 °C,
Time 252000 sec
674 %
@Temperature 302 °F,
Time 70.0 hour
ASTM Oil #1
 726.9 %
@Temperature 150 °C,
Time 252000 sec
726.9 %
@Temperature 302 °F,
Time 70.0 hour
Heat Aged
100% Modulus 0.359 MPa52.0 psi
Tear Strength 10.5 kN/m60.0 pliDie C
 35.8 kN/m204 pliDie B
Compression Set 12.8 %
@Temperature 100 °C,
Time 79200 sec
12.8 %
@Temperature 212 °F,
Time 22.0 hour
Solid
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature <= -69.4 °C<= -93.0 °F
 
Descriptive Properties
ColorSalmon

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL155 / 318365

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.