UBE 1015RXN Polyamide 6, Mineral Filled
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 40% Mineral Filled
Material Notes:
Characteristic: Injection, reinforced with mineral fillers 35%, good surface finish.
Information provided by UBE Industries, LTD
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.40
g/cc
0.0506
lb/in³
ISO 1183-3
Moisture Absorption
1.70 %
1.70 %
50% RH; UBE method
Linear Mold Shrinkage, Flow
0.0030
cm/cm
@Thickness 3.00 mm
0.0030
in/in
@Thickness 0.118 in
30x100x3t; UBE method
Linear Mold Shrinkage, Transverse
0.0050
cm/cm
@Thickness 3.00 mm
0.0050
in/in
@Thickness 0.118 in
30x100x3t; UBE method
Mechanical Properties
Metric
English
Comments
Tensile Strength
80.0
MPa
11600
psi
ISO 527-1,2
Elongation at Break
2.5 %
2.5 %
ISO 527-1,2
Tensile Modulus
8.20
GPa
1190
ksi
ISO 527-1,2
Flexural Strength
125
MPa
18100
psi
ISO 178
Flexural Modulus
7.70
GPa
1120
ksi
ISO 178
Charpy Impact, Notched
0.200
J/cm²
0.952
ft-lb/in²
ISO 179-1/1eA
Thermal Properties
Metric
English
Comments
Melting Point
215
-
225
°C
419
-
437
°F
ISO 11357
Deflection Temperature at 1.8 MPa (264 psi)
145
°C
293
°F
ISO 75-1,2
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PUBD9818 / 287281
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.