MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

LyondellBasell Moplen HP400N Polypropylene Homopolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Molded

Material Notes: Description: HP400N is a high flow homopolymer with a conventional molecular weight distribution and is formulated with a general-purpose additive package. HP400N is designed for injection molding applications where ease of flow is important. It may also be used in conjunction with selected fillers. All ingredients in HP400N meet the chemical registration requirements of TSCA (U.S.) and DSL (Canada). Uses: Medical applications, packaging, containers

Information provided by Basell.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM D792 & ISO 1183
Melt Flow  11 g/10 min
@Load 2.16 kg,
Temperature 230 °C
11 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1183
 12 g/10 min
@Load 2.16 kg,
Temperature 230 °C
12 g/10 min
@Load 4.76 lb,
Temperature 446 °F
Condition L; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 9393ASTM D 785
Hardness, Shore D 7373ISO 868
Tensile Strength, Yield 32.0 MPa4640 psiISO 527-1, -2
 35.2 MPa5100 psiASTM D 638
Elongation at Yield 9.0 %9.0 %ASTM D 638
Flexural Modulus 1.40 GPa203 ksiISO 178
Flexural Modulus, 1% Secant 1590 MPa230000 psi0.05 in/min; ASTM D790
Izod Impact, Notched 0.320 J/cm0.600 ft-lb/in73°F; ASTM D256
Izod Impact, Notched (ISO) 2.50 kJ/m²1.19 ft-lb/in²Type 1, Notch A; ISO 180
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 93.3 °C200 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 51.1 °C124 °FUnannealed; ISO 75A-1, -2
Vicat Softening Point 155 °C311 °FMethod A; ISO 306
UL RTI, Electrical 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
UL RTI, Mechanical with Impact 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
UL RTI, Mechanical without Impact 221 °C
@Thickness 0.711 mm
430 °F
@Thickness 0.0280 in
UL 746
Flammability, UL94 HB
@Thickness 0.711 mm
HB
@Thickness 0.0280 in
NC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Astryn SB572C Polypropylene Copolymer
LyondellBasell Moplen HP400L Polypropylene Homopolymer
Chi Mei Polylac® PA-757 ABS
PolyMirae Moplen EP548P Injection Molding Grade Polypropylene
LyondellBasell Astryn 65F5-4 Polypropylene Homopolymer, 40% Calcium Carbonate

PMO843 / 53832

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.