MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Herculoy®, High-Silicon Bronze A, UNS C65500, H02 Temper, Flat Products, Rod & Bar
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Temper: 1/2 Hard

Fabrication Properties: Excellent Suitability – Brazing, Gas Shielded Arc Welding, Spot Weld, Seam Weld, Butt Weld, Capacity for Being Cold Worked, Capacity for Being Hot Formed; Good Suitability – Soldering, Oxyacetylene Welding; Fair Suitability – Coated Metal Arc Welding

Common Fabrication Processes: Blanking; Drawing; Forming and Bending; Heading and Upsetting; Hot Forging and Pressing; Roll Threading and Knurling; Shearing; Squeezing and Swaging

Typical uses: Sculpture; Motors, Rotor Bar; Pole Line Hardware; Bolts; Clamps; Cotter Pins; Hinges; Nails; Rivets; Screws; Bearing Plates; Bushings; Butts; Cable; Channels; Chemical Equipment; Doctor Blades, Paper Industry; Heat Exchanger Tubes; Hydraulic Pressure Lines; Kettles; Oil Refinery Plumbing Tube; Piston Rings; Pressure Vessels; Screen Cloth; Screen Plates; Shafting; Tanks; Wear Plates; Welded Pressure Vessels; Welded Tanks; Wire; Hardware; Propeller Shafts

Applicable Specifications: Bar – B124/B124M, SAE J461, SAE J463; Bolts – ASTM F468; Forgings, Die (Hot Pressed) – ASME SB283, ASTM B283/B283M; Nuts – ASTM F467; Plate - Bridge and Bearing ASTM B100; Rod – SAE J463, Forgings ASTM B124/B124M, SAE J461; Rod, Bar & Shapes - Copper-Silicon Alloy ASTM B98/B98M, Copper-Silicon Alloy ASME SB98; Screws – ASTM F468; Seamless Pipe and Tube – ASTM B315, ASME SB315; Shapes – SAE J463, Forgings ASTM B124/B124M, SAE J461; Sheet – SAE J461, SAE J463, Bridge and Bearing ASTM B100; Sheet, Strip, Roller Bar & Plate - for Pressure Vessels & General Purpose ASTM B96/B96M, for Pressure Vessels & General Purpose ASME SB96; Strip – SAE J463, SAE J461; Studs – ASTM F468; Tube – MILITARY MIL-T-8231; Wire – ASTM B99/B99M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.53 g/cc0.308 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  538 MPa
@Thickness 25.4 mm
78000 psi
@Thickness 1.00 in
 538 MPa
@Thickness 1.02 mm
78000 psi
@Thickness 0.0400 in
 676 MPa
@Thickness 2.03 mm
98000 psi
@Thickness 0.0800 in
Tensile Strength, Ultimate  345 MPa
@Thickness 1.02 mm
50000 psi
@Thickness 0.0400 in
 359 MPa
@Thickness 25.4 mm
52000 psi
@Thickness 1.00 in
 400 MPa
@Thickness 2.03 mm
58000 psi
@Thickness 0.0800 in
Tensile Strength, Yield  310 MPa
@Thickness 25.4 mm
45000 psi
@Thickness 1.00 in
0.5% Ext
 310 MPa
@Thickness 1.02 mm
45000 psi
@Thickness 0.0400 in
0.5% Ext
Elongation at Break  8.0 %
@Thickness 2.03 mm
8.0 %
@Thickness 0.0800 in
 17 %
@Thickness 1.02 mm
17 %
@Thickness 0.0400 in
 35 %
@Thickness 25.4 mm
35 %
@Thickness 1.00 in
Tensile Modulus 103 GPa15000 ksi
Modulus of Rigidity 38.6 GPa5600 ksi
Poissons Ratio 0.340.34Calculated
Machinability 30 %30 %
Forgeability 40 %40 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000250 ohm-cm0.0000250 ohm-cm7% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 µm/m-°C
@Temperature 20.0 - 300 °C
10.0 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 3.03 W/m-K21.0 BTU-in/hr-ft²-°F
Melting Point 971 - 1030 °C1780 - 1880 °F
Solidus 971 °C1780 °F
Liquidus 1030 °C1880 °F
Annealing Point 482 - 704 °C900 - 1300 °F
 
Processing PropertiesMetricEnglishComments
Hot-Working Temperature 704 - 871 °C1300 - 1600 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 92 - 96.7 %92 - 96.7 %As Balance
Iron, Fe <= 0.80 %<= 0.80 %
Lead, Pb <= 0.050 %<= 0.050 %
Manganese, Mn 0.50 - 1.3 %0.50 - 1.3 %
Nickel, Ni <= 0.60 %<= 0.60 %
Silicon, Si 2.8 - 3.8 %2.8 - 3.8 %
Zinc, Zn <= 1.5 %<= 1.5 %
 
Descriptive Properties
Cold Work (%)201 in
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC65500x3 / 293061

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.