MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
BASF Ultramid® Advanced T1000 HG7 LS BK23593 Polyphthalamide, 35% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 40% Glass Fiber Reinforced

Material Notes: Ultramid Advanced T1000 HG7 LS BK23593 is a heat stabilized, partially aromatic, 35% glass fiber reinforced polyphthalamide for injection molding with strong mechanical properties especially at elevated temperatures and excellent chemical resistance for highly stressed parts. This material has high strength and stiffness, very low water absorption and outstanding dimensional stability. It features a high melting point (320C) and excellent melt stability. This grade is suitable for laser marking.

Information provided by BASF.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.485 g/ccISO 1183
Moisture Absorption 1.60 %50% RH; ISO 62
Water Absorption at Saturation 3.8 %ISO 62
Linear Mold Shrinkage, Flow 0.0040 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0093 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 135 MPa
@Temperature 120 °C
Dry; ISO 527
 145 MPa
@Temperature 80.0 °C
Conditioned; ISO 527
 180 MPa
@Temperature 80.0 °C
Dry; ISO 527
 210 MPa
@Temperature 23.0 °C
Conditioned; ISO 527
 220 MPa
@Temperature 23.0 °C
Dry; ISO 527
Elongation at Break 1.9 %
@Temperature 23.0 °C
Conditioned; ISO 527
 2.0 %
@Temperature 23.0 °C
Dry; ISO 527
 2.0 %
@Temperature 80.0 °C
Dry; ISO 527
 2.2 %
@Temperature 80.0 °C
Conditioned; ISO 527
 2.9 %
@Temperature 120 °C
Dry; ISO 527
Tensile Modulus 10000 MPa
@Temperature 120 °C
Dry; ISO 527
 12000 MPa
@Temperature 80.0 °C
Conditioned; ISO 527
 12500 MPa
@Temperature 80.0 °C
Dry; ISO 527
 14000 MPa
@Temperature 23.0 °C
Dry; ISO 527
 14000 MPa
@Temperature 23.0 °C
Conditioned; ISO 527
Charpy Impact Unnotched 70.0 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179
 70.0 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179
Charpy Impact, Notched 8.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179
 8.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmConditioned; IEC 60093
 >= 1.00e+15 ohm-cmDry; IEC 60093
Dielectric Strength 37.0 kV/mmDry; IEC 60243-1
 
Thermal PropertiesOriginal ValueComments
Melting Point 320 °CDry; ISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 280 °CDry; ISO 75
UL RTI, Electrical 85.0 °C
@Thickness 0.750 mm
UL746B
 85.0 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical with Impact 85.0 °C
@Thickness 0.750 mm
UL746B
 85.0 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical without Impact 85.0 °C
@Thickness 0.750 mm
UL746B
 85.0 °C
@Thickness 3.00 mm
UL746B
Flammability, UL94 HB
@Thickness 0.750 mm
 HB
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 345 - 360 °C
Mold Temperature 150 - 170 °C
Drying Temperature 120 °C
@Time 28800 sec
Moisture Content <= 0.050 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASF8958 / 254916

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.