MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC SABIC® STAMAX™ 30YK270E PP (Global)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: SABIC® STAMAX 30YK270E is a 30% long glass fiber reinforced low emission grade with improved impact and flow properties. The glass fibres are chemically coupled to the PP matrix, resulting in high stiffness and strength. IMDS ID: 80929807

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.12 g/cc0.0405 lb/in³ISO 1183
Filler Content 30 %30 %Glass Fiber Content; ISO 3451
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 100 MPa14500 psiISO 527/1A
 55.0 MPa
@Temperature 80.0 °C
7980 psi
@Temperature 176 °F
ISO 527/1A
Elongation at Break 2.4 %2.4 %ISO 527/1A
Tensile Modulus 6.20 GPa899 ksiISO 527/1A
 4.40 GPa
@Temperature 80.0 °C
638 ksi
@Temperature 176 °F
ISO 527/1A
Flexural Strength 150 MPa21800 psiISO 178
 75.0 MPa
@Temperature 80.0 °C
10900 psi
@Temperature 176 °F
ISO 178
Flexural Modulus 6.00 GPa870 ksiISO 178
 4.00 GPa
@Temperature 80.0 °C
580 ksi
@Temperature 176 °F
ISO 178
Charpy Impact Unnotched 6.00 J/cm²28.6 ft-lb/in²ISO 179/1eU
 7.50 J/cm²35.7 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 2.80 J/cm²13.3 ft-lb/in²ISO 179/1eA
 2.80 J/cm²13.3 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear 40.0 µm/m-°C
@Temperature -30.0 - 100 °C
22.2 µin/in-°F
@Temperature -22.0 - 212 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 158 °C316 °FISO 75/A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI11562 / 245029

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.