MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Asahi Kasei Xyron® 740V Modified Polyphenylene Ether  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polyphenylene Ether, Heat Resistant

Material Notes: Flame Retardant

Information provided by Asahi Kasei

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.08 g/cc23°C; ASTM D792
Moisture Absorption 0.100 %23°C, 50% RH 24 hours; ASTM D570
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 71.0 MPa23°C, 50% RH; ASTM D638
Elongation at Break 40 %23°C, 50% RH; ASTM D638
Flexural Strength 107 MPa23°C, 50% RH; ASTM D790
Flexural Modulus 2.55 GPa23°C, 50% RH; ASTM D790
Izod Impact, Notched 147 J/m
@Thickness 6.40 mm,
Temperature 23.0 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cm50% RH; ASTM D257
Surface Resistance 1.00e+16 ohm50% RH; ASTM D257
Dielectric Constant 2.9
@Frequency 1e+6 Hz
50% RH; ASTM D150
 2.9
@Frequency 1e+6 Hz
50% RH; ASTM D150
Dielectric Strength 29.0 kV/mm
@Thickness 2.00 mm
Short time; ASTM D149
Dissipation Factor 0.0030
@Frequency 60 Hz
50% RH; ASTM D150
 0.0040
@Frequency 1e+6 Hz
50% RH; ASTM D150
Arc Resistance 70 secTungsten; ASTM D495
 
Thermal PropertiesOriginal ValueComments
CTE, linear 70.0 µm/m-°C
@Temperature -30.0 - 60.0 °C
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 140 °CASTM D648
Flammability, UL94 V-1
@Thickness 1.60 mm
 V-1
@Thickness 3.20 mm
 
Processing PropertiesOriginal ValueComments
Processing Temperature 240 - 300 °CResin Temperature
Mold Temperature 60.0 - 100 °C
Drying Temperature 90.0 - 100 °CPre-drying Temperature
Dry Time 2 - 4 hour

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
American Polymers API 375 Polystyrene
Asahi Kasei Xyron® X9653 Modified Polyphenylene Ether
Asahi Kasei Xyron® X5403 PPE/PA
Asahi Kasei Xyron® X0700 Modified Polyphenylene Ether
Asahi Kasei Xyron® 450H Modified Polyphenylene Ether

PASAHI069 / 24680

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.