MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Chemours Teflon™ PFA 951HP Plus Premium fluoropolymer resin
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA); Polyperfluoroalkoxyethylene, Molded/Extruded

Material Notes: Teflon™ PFA 951HP Plus is a premium fluoropolymer resin available in pellet form. Teflon™ PFA 951HP Plus possesses the same exceptional chemical resistance, high purity, and protection against ionic contamination as Teflon™ PFA HP grades with the added benefits of improved flex life and chemical stress-crack resistance. Teflon™ PFA 951HP Plus has unmatched HCl permeation resistance, and is also 45% less permeable to nitrogen than other PFAs (permeation by nitrogen is a general indication of the rate of permeation by other molecules). Additionally, the improved flex life and chemical resistance will reduce the cost of ownership of high purity fluid handling systems by reducing downtime caused by mechanical or chemical stresses. Parts molded with Teflon™ PFA 951HP Plus have an exceptionally smooth finish, which can further help prevent buildup of microbial contamination in water handling systems. With permeation resistance that is up to 60% greater than standard PFA, Teflon™ PFA 951HP Plus is designed for applications where reduced chemical permeation, resistance to stress-cracking, and surface smoothness are critical to reducing contamination and protecting process yields. Applications for Teflon™ PFA 951HP Plus include fluid handling components for high performance chemical delivery systems, as well as tubing, unsupported pipe linings for the production of ultra-pure chemicals, and semiconductor components where purity in the parts-per-billion range is needed.

Information provided by Chemours.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.15 g/ccASTM D792
Water Absorption <= 0.030 %
@Time 86400 sec
ASTM D570
Melt Flow 2.0 g/10 minASTM D3307
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 55ASTM D2240
Tensile Strength 15.0 MPa
@Temperature 200 °C
ASTM D3307
 28.0 MPa
@Temperature 23.0 °C
ASTM D3307
Elongation, Ultimate 290 %
@Temperature 23.0 °C
ASTM D3307
 450 %
@Temperature 200 °C
ASTM D3307
Flexural Modulus 0.0550 GPa
@Temperature 200 °C
ASTM D790
 0.600 GPa
@Temperature 23.0 °C
ASTM D790
Flex Crack Resistance 1.80e+6
@Thickness 0.203 mm
Cycles MIT Folding Endurance; ASTM D2176
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+18 ohm-cmASTM D257
Surface Resistivity per Square >= 1.00e+17 ohmASTM D257
Dielectric Constant 2.03
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 80.0 kV/mm
@Thickness 0.250 mm
Short Time; ASTM D149
Dissipation Factor 0.00020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance >= 180 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Melting Point 300 - 320 °CASTM D4591
Flammability, UL94 V-0
Oxygen Index >= 95 %ASTM D2863
 
Descriptive Properties
Chemical/Solvent ResistanceExcellentASTM D543
Critical Shear Rate (1/s)12372°C
Heat of Combustion5.3 MJ/kgASTM D240
Salt Spray Resistance Coatings (hours)1000ASTM B117. 5% NaCl at 35 °C (95 °F).
Weather and Chemical ResistanceOutstanding
Weather Resistance (years unaffected)10Florida Exposure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDU8810 / 268736

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.