MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Norplex-Micarta EndurX™ BP13HPM Phenolic Cotton Laminate Sheet, MoS2 Lubricated
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Phenolic

Material Notes: Canvas phenolic laminate with molybdenum disulfide added as a solid lubricant. This material has improved wear properties under certain conditions. Material is semi-conductive to electricity and should no be used where this is detrimental to the application.

Key Words: Cotton, Phenolic, Micarta, Molybdenum Disulfide Lubricant
Vendors: Norplex-Micarta is the leading manufacturer of high performance thermoset composite materials. We work directly with customers to manufacture the highest quality specialty sheet products, pre-pregs, rods and molded shapes, and tubes to meet demanding composite applications for our OEMs and fabricators around the world. Visit norplex-micarta.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.40 g/ccASTM D792
Moisture Absorption 1.50 %Condition A; ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 100ASTM D785
Tensile Strength 9000 psi
@Thickness 3.17 mm
Condition A, Crosswise; ASTM D638
 16000 psi
@Thickness 3.17 mm
Condition A, Lengthwise; ASTM D638
Flexural Strength 19500 psi
@Thickness 1.57 mm
Condition A, Crosswise; ASTM D790
 26000 psi
@Thickness 1.57 mm
Condition A, Lengthwise; ASTM D790
Flexural Modulus 1000 ksi
@Thickness 1.57 mm
Condition A, Crosswise; ASTM D790
 1200 ksi
@Thickness 1.57 mm
Condition A, Lengthwise; ASTM D790
Compressive Strength 49000 psi
@Thickness 12.7 mm
Condition A, Flatwise; ASTM D695
Shear Strength 13500 psi
@Thickness 1.57 mm
Condition A, Perpendicular; ASTM D732
Adhesive Bond Strength 2300 psi
@Thickness 12.7 mm
Condition A, Bonding Strength; ASTM D229
Izod Impact, Notched 2.70 ft-lb/in
@Thickness 12.7 mm
Condition E-48/50, Crosswise; ASTM D256
 3.50 ft-lb/in
@Thickness 12.7 mm
Condition E-48/50, Lengthwise; ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.0 µm/m-°C
@Thickness 3.17 mm
X-axis; IPC-TM 650-2.4.24
 15.0 µm/m-°C
@Thickness 3.17 mm
Y-axis; IPC-TM 650-2.4.24
UL RTI, Mechanical without Impact 145 °CUL Bulletin 746b
Flammability, UL94 HB
@Thickness 1.57 mm
Condition A
 
Descriptive Properties
SubstrateCotton

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PNORPM230 / 280546

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.