MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

BASF Ultramid® A 218 V50 Black 21N Nylon 66, 33% Glass Fiber Reinforced, Heat Stabilized, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled; Nylon 66, Heat Stabilized

Material Notes: Product Description: Ultramid® A 218 V50 Black 21N is a polyamide 66, reinforced with 50% of glass fiber, heat stabilized, for injection molding. This grade offers an excellent combination between thermal and mechanical properties.

Availability: Africa & Middle East; Asia Pacific; Latin America; North America

Filler/Reinforcement: Glass Fiber, 50% Filler by Weight

Features: Good Flow; Good Mold Release; Heat Stabilized – Inorganic; High Stiffness

Use: Automotive Applications; Consumer Applications; Industrial Applications

Agency Ratings: EC 1907/2006 (REACH)

RoSH Compliance: RoSH Compliant

Appearance: Black; Natural Color

Forms: Pellets

Processing Method: Injection Molding

Resin ID (ISO 1043): PA66-GF50

Information provided by BASF Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.55 g/cc0.0560 lb/in³ISO 1183
Maximum Moisture Content 0.200.20
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 175 MPa25400 psiISO 527-2
Elongation at Break 4.0 %4.0 %ISO 527-2
Tensile Modulus 12.5 GPa1810 ksiISO 527-1
Flexural Modulus 10.0 GPa1450 ksiISO 178
Izod Impact, Notched (ISO) 17.0 kJ/m²8.10 ft-lb/in²ISO 180/A
Charpy Impact Unnotched 9.45 J/cm²45.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.81 J/cm²8.60 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 62631-3-1
Surface Resistance 1.00e+12 ohm1.00e+12 ohmIEC 62631-3-2
Dielectric Constant 4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 29.9 kV/mm
@Thickness 2.00 mm
760 kV/in
@Thickness 0.0787 in
IEC 60243-1
Dissipation Factor 0.11
@Frequency 100 Hz
0.11
@Frequency 100 Hz
IEC 62631-2-1
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 270 - 280 °C518 - 536 °F
Middle Barrel Temperature 280 - 290 °C536 - 554 °F
Front Barrel Temperature 280 - 300 °C536 - 572 °F
Mold Temperature 70.0 - 100 °C158 - 212 °F
Drying Temperature 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASG2091 / 310784

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.