MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC XENOY™ FR Resin ENH2900 Polycarbonate + PBT (PC+PBT) (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Unreinforced

Material Notes: XENOY ENH2900 resin is a Non-Braominated, Non Chlorinated flame retarded PC/PBT resin with good flow, high impact and excellent chemical resistance. It was designed quite suitable for E&E housing applications

Features: Flame Retardant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Moisture Absorption 0.0400 %0.0400 %Injection Molding
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 26 g/10 min
@Load 5.00 kg,
Temperature 266 °C
26 g/10 min
@Load 11.0 lb,
Temperature 511 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 42.0 MPa6090 psi50 mm/min; ASTM D638
Tensile Strength, Yield 63.0 MPa9140 psi50 mm/min; ASTM D638
Elongation at Break 65 %65 %50 mm/min; ASTM D638
Elongation at Yield 4.0 %4.0 %50 mm/min; ASTM D638
Tensile Modulus 2.48 GPa360 ksi50 mm/min; ASTM D638
Flexural Strength 89.0 MPa12900 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.24 GPa325 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 550 J406 ft-lbASTM D256
Dart Drop, Total Energy 65.0 J47.9 ft-lbASTM D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 78.0 °C
@Thickness 3.20 mm
172 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 102 °C216 °FRate B/50; ASTM D1525
UL RTI, Electrical 75.0 °C167 °FUL 746B
UL RTI, Mechanical with Impact 75.0 °C167 °FUL 746B
UL RTI, Mechanical without Impact 75.0 °C167 °FUL 746B
Flammability, UL94  HB
@Thickness >=0.400 mm
HB
@Thickness >=0.0157 in
UL 94
 V-1
@Thickness >=1.10 mm
V-1
@Thickness >=0.0433 in
UL 94
 V-0
@Thickness >=1.50 mm
V-0
@Thickness >=0.0591 in
UL 94
 5VB
@Thickness >=2.50 mm
5VB
@Thickness >=0.0984 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 245 - 275 °C473 - 527 °F
Zone 2 220 - 265 °C428 - 509 °F
Zone 3 245 - 275 °C473 - 527 °F
Melt Temperature 245 - 275 °C473 - 527 °FInjection Molding
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Drying Temperature 80.0 - 90.0 °C176 - 194 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 30 - 80 %30 - 80 %
Vent Depth 0.00380 - 0.00760 cm0.00150 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82793 / 290740

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.