MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Chemours Teflon™ PFA 345 Medium melt flow rate fluoropolymer resin
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Teflon™ PFA 345 is a medium melt flow rate fluoropolymer resin available in pellet form. Compared with Teflon™ PFA 340, it offers increased flex life and greater resistance to environmental stress-cracking (Teflon™ PFA 345 offers a typical MIT folding endurance of 50,000* compared to 15,000 in Teflon™ PFA 340). Applications for Teflon™ PFA 345 include extruded tubing, wire and cable insulation, injection molded parts, and chemically resistant linings for bellows, valves, fittings, pipes, pumps, and other fluid-handling components.

Information provided by Chemours.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.15 g/ccASTM D792
Water Absorption <= 0.030 %
@Time 86400 sec
ASTM D570
Melt Flow 5.0 g/10 minASTM D3307
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 55ASTM D2240
Tensile Strength 27.0 MPaASTM D3307
Elongation, Ultimate 300 %ASTM D3307
Flexural Modulus 0.551 GPaASTM D790
Flex Crack Resistance 50000
@Thickness 0.203 mm
Cycles MIT Folding Endurance; ASTM D2176
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+18 ohm-cmASTM D257
Surface Resistivity per Square >= 1.00e+17 ohmASTM D257
Dielectric Constant 2.03
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 80.0 kV/mm
@Thickness 0.250 mm
Short Time; ASTM D149
Dissipation Factor 0.00020
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance >= 180 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Melting Point 305 °CASTM D4591
Maximum Service Temperature, Air 260 °CContinuous, per accelerated heat-aging test
Flammability, UL94 V-0
Oxygen Index >= 95 %ASTM D2863
 
Descriptive Properties
Chemical/Solvent ResistanceExcellentASTM D543
Critical Shear Rate (1/s)21372°C
Heat of Combustion5.3 MJ/kgASTM D240
Salt Spray Resistance Coatings (hours)1000ASTM B117. 5% NaCl at 35 °C (95 °F).
Weather and Chemical ResistanceOutstanding
Weather Resistance (years unaffected)10Florida Exposure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDU8800 / 268726

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.