MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Ajedium™ Film - Halar® 500LC ECTFE
Categories: Polymer; Film; Thermoplastic; Fluoropolymer; ETFE/ECTFE; ECTFE Fluoropolymer

Material Notes: ECTFE film, strong, tough, abrasion resistant with excellent weathering properties

Halar® ECTFE is a semi-crystalline fluoropolymer with a chemical structure of a 1:1 alternating copolymer of ethylene and chlorotrifluoroethylene.

Halar® film is a strong, hard, tough, abrasion resistant film that retains its useful properties over a broad range of temperatures. Its low temperature properties, especially those related to impact, are particularly outstanding.

Halar® films have demonstrated excellent weathering properties and are extremely resistant to UV radiation and common industrial and environmental pollutants. The film also is an excellent barrier to water vapor at a wide range of temperatures. This lower permeability is a key advantage in applications where protection from water, oxygen, or other small gas molecules is required.

Applications: Aerospace Applications; Electrical/Electronic Applications; Industrial Applications; Outdoor Applications

Features: Low Viscosity

Standard Thicknesses and Widths
- Widths are available from 22" (559 mm) to 56" (1422 mm).
- Products with widths <22 inches or >56 inches are available upon request.
- Tolerances for widths are +/- 4mm.
- For Halar® film, the standard thicknesses are 8 microns (0.3 mil) to 1016 microns (40 mil).

Surface Finishes
- Standard surface finish is P/M (polished / matte).
- Custom finishes of P/P (polished / polished) and M/M (matte / matte) are available.

Packaging
- Film is supplied in a roll form of high quality, cardboard core of 3" (76mm) or 6" (152mm).
- PVC cores are available upon request in 3" and 6" sizes.

Labeling
- Products are labeled to comply with national and international standards.
- Labels include product grade, unique batch number, roll length, roll width, product thickness, and net weight.

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.68 g/ccASTM D792
Water Absorption at Saturation <= 0.10 %ASTM D570
Moisture Vapor Transmission 1.60 cc-mm/m²-24hr-atmASTM F1249
Thickness 50.0 micronsAs Tested
 50.0 micronsAs Tested
 125 micronsAs Tested
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 34.5 MPaASTM D882
Film Elongation at Break, MD 280 %ASTM D882
Film Elongation at Break, TD 280 %ASTM D882
Film Elongation at Yield, MD 6.0 %ASTM D882
Secant Modulus, MD 1.55 GPaASTM D882
Secant Modulus, TD 1.50 GPaASTM D882
Coefficient of Friction, Dynamic 0.20vs. Itself; ASTM D1894
Coefficient of Friction, Static 0.20vs. Itself; ASTM D1894
Dart Drop Test 610 gMethod A; ASTM D1709
Taber Abrasion, mg/1000 Cycles 5.0CS-10 Wheel, 1000 g, 1000 Cycles; ASTM D1044
Film Tensile Strength at Break, MD 53.0 MPaASTM D882
Film Tensile Strength at Break, TD 50.0 MPaASTM D882
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 5.50e+16 ohm-cmASTM D257
Dielectric Constant 2.57
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 14.0 kV/mm
@Thickness 3.20 mm
ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 100 µm/m-°CASTM D696
Specific Heat Capacity 0.962 J/g-°CASTM C351
Thermal Conductivity 0.150 W/m-K
@Temperature 40.0 °C
ASTM C177
Melting Point 242 °C
Crystallization Temperature 222 °CPeak; ASTM D3418
Brittleness Temperature <= -76.0 °CProcedure A; ASTM D746
Glass Transition Temp, Tg 85.0 °CASTM E1356
Oxygen Index 52 %ASTM D2863
Shrinkage 4.4 %
@Temperature 200 °C
Free Shrinkage; ASTM D2732
 
Descriptive Properties
Area Factor115 ft²/lb/mil
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorClear/Transparent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4002 / 279802

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.